FabDigit

S7 vs 4130 and 2 more: properties

S7413043408620

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

207 GPa30 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi

Tensile Strength (Ultimate)

830 MPa120 ksi
700 MPa102 ksi
950 MPa138 ksi
635 MPa92.1 ksi

Yield Strength (0.2% offset)

530 MPa76.9 ksi
440 MPa63.8 ksi
620 MPa89.9 ksi
385 MPa55.8 ksi

Elongation at Break

18%
22%
18%
28%

Reduction in Area

42%
50%
45%
60%

Compressive Strength

545 MPa79 ksi
480 MPa69.6 ksi
640 MPa92.8 ksi

Shear Strength

500 MPa72.5 ksi
440 MPa63.8 ksi
580 MPa84.1 ksi
390 MPa56.6 ksi

Fatigue Strength (Endurance Limit)

380 MPa55.1 ksi
330 MPa47.9 ksi
430 MPa62.4 ksi
295 MPa42.8 ksi

Fracture Toughness (K_IC)

95 MPa·√m86.5 ksi·√in
110 MPa·√m100 ksi·√in
95 MPa·√m86.5 ksi·√in
85 MPa·√m77.4 ksi·√in

Charpy V-Notch Impact (RT)

65 J47.9 ft·lbf
55 J40.6 ft·lbf
30 J22.1 ft·lbf
90 J66.4 ft·lbf

Hardness, Brinell

200 HB
210 HB
285 HB
183 HB

Hardness, Rockwell B

94 HRB
95 HRB
100 HRB
90 HRB

Hardness, Rockwell C

15 HRC
29 HRC

Hardness, Vickers

210 HV
228 HV
300 HV

Same in both: Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Density

7.83 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,420°C2,588 °F
1,432°C2,610 °F
1,416°C2,581 °F
1,425°C2,597 °F

Liquidus Temperature

1,480°C2,696 °F
1,510°C2,750 °F
1,454°C2,649 °F
1,505°C2,741 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

26 W/m·K15 BTU/hr·ft·°F
42.7 W/m·K24.7 BTU/hr·ft·°F
44.5 W/m·K25.7 BTU/hr·ft·°F
46.6 W/m·K26.9 BTU/hr·ft·°F

Specific Heat Capacity

460 J/kg·K0.11 BTU/lb·°F
477 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.6 µm/m·K7 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
11.6 µm/m·K6.4 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
272 J/g117 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb

Max Service Temperature (continuous)

500°C932 °F
400°C752 °F
400°C752 °F
400°C752 °F

Min Service Temperature

-40°C-40 °F
-50°C-58 °F
-40°C-40 °F
-40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

2.9 % IACS
7.7 % IACS
7 % IACS
8 % IACS

Electrical Resistivity

6×10⁻⁷ Ω·m23.6 µΩ·in
2.23×10⁻⁷ Ω·m8.78 µΩ·in
2.48×10⁻⁷ Ω·m9.76 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

18 / 100
14 / 100
12 / 100
11 / 100

Galvanic Potential (seawater, vs SCE)

-0.61 V
-0.62 V
-0.6 V

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

50 / 100
55 / 100
48 / 100
62 / 100

Machinability Rating (AISI 1212 = 100 %)

50%
60%
50%
65%

Weldability

30 / 100
65 / 100
33 / 100
60 / 100

Formability (cold)

35 / 100
45 / 100
35 / 100
55 / 100

Brazeability / Solderability

40 / 100
70 / 100
55 / 100
65 / 100

Polishability

75 / 100
60 / 100
70 / 100
70 / 100

Castability

45 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

36 MJ/kg15,477 BTU/lb
30 MJ/kg12,898 BTU/lb
32 MJ/kg13,758 BTU/lb
30 MJ/kg12,898 BTU/lb

Embodied Carbon (primary production)

2.7 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.1 kg CO₂/kg

Embodied Water

65 L/kg7.8 gal/lb
45 L/kg5.4 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

40%
30%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

106 kN·m/kg
89 kN·m/kg
121 kN·m/kg
81 kN·m/kg

Specific Stiffness (E / density)

26.4 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

679 kJ/m³
472 kJ/m³
938 kJ/m³
362 kJ/m³

Thermal Diffusivity

7.2 mm²/s
11.4 mm²/s
11.9 mm²/s
12.5 mm²/s

Thermal Shock Resistance Index

8
12
17
12

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale413043408620S7

Manufacturing and finishing

CapabilityS7413043408620
Sheet metalYesYesYes
Default conditionAnnealedHRHRHR
Relative cost$$$$$ Specialty$$ Standard$$$ Premium$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in S7 and 4130 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.