Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

210 GPa30.5 Msi
200 GPa29 Msi
200 GPa29 Msi
206 GPa29.9 Msi

Shear Modulus

81 GPa11.7 Msi
79 GPa11.5 Msi
79.3 GPa11.5 Msi
79 GPa11.5 Msi

Poisson's Ratio

0.3
0.29
0.29
0.3

Tensile Strength (Ultimate)

420 MPa60.9 ksi
420 MPa60.9 ksi
450 MPa65.3 ksi
420 MPa60.9 ksi

Yield Strength (0.2% offset)

260 MPa37.7 ksi
230 MPa33.4 ksi
260 MPa37.7 ksi
250 MPa36.3 ksi

Elongation at Break

26%
25%
22%
28%

Reduction in Area

55%
45%
50%
55%

Compressive Strength

255 MPa37 ksi
230 MPa33.4 ksi
260 MPa37.7 ksi
250 MPa36.3 ksi

Shear Strength

260 MPa37.7 ksi
270 MPa39.2 ksi
275 MPa39.9 ksi
260 MPa37.7 ksi

Fatigue Strength (Endurance Limit)

170 MPa24.7 ksi
190 MPa27.6 ksi
200 MPa29 ksi
190 MPa27.6 ksi

Fracture Toughness (K_IC)

80 MPa·√m72.8 ksi·√in
90 MPa·√m81.9 ksi·√in
100 MPa·√m91 ksi·√in
110 MPa·√m100 ksi·√in

Charpy V-Notch Impact (RT)

40 J29.5 ft·lbf
27 J19.9 ft·lbf
55 J40.6 ft·lbf
45 J33.2 ft·lbf

Hardness, Rockwell B

67 HRB
68 HRB
67 HRB
67 HRB

Hardness, Vickers

125 HV
126 HV
126 HV
126 HV

Same in both: Bulk Modulus 160 GPa23.2 Msi · Hardness, Brinell 120 HB

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,425°C2,597 °F
1,425°C2,597 °F
1,470°C2,678 °F
1,495°C2,723 °F

Liquidus Temperature

1,520°C2,768 °F
1,510°C2,750 °F
1,520°C2,768 °F
1,520°C2,768 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

50 W/m·K28.9 BTU/hr·ft·°F
51 W/m·K29.5 BTU/hr·ft·°F
51.9 W/m·K30 BTU/hr·ft·°F
50 W/m·K28.9 BTU/hr·ft·°F

Specific Heat Capacity

460 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
486 J/kg·K0.12 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12 µm/m·K6.7 µin/in·°F
11.7 µm/m·K6.5 µin/in·°F
11.7 µm/m·K6.5 µin/in·°F
12 µm/m·K6.7 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
247 J/g106 BTU/lb
247 J/g106 BTU/lb
270 J/g116 BTU/lb

Max Service Temperature (continuous)

350°C662 °F
400°C752 °F
400°C752 °F
350°C662 °F

Min Service Temperature

0°C32 °F
-20°C-4 °F
-20°C-4 °F
-20°C-4 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

11 % IACS
10.8 % IACS
11 % IACS
10.8 % IACS

Same in both: Electrical Resistivity 1.6×10⁻⁷ Ω·m6.3 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.61 V
-0.65 V
-0.65 V
-0.63 V

Same in both: Corrosion Resistance 10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

66 / 100
65 / 100
65 / 100
65 / 100

Machinability Rating (AISI 1212 = 100 %)

65%
70%
72%
70%

Formability (cold)

85 / 100
78 / 100
80 / 100
85 / 100

Castability

40 / 100
40 / 100

Brazeability / Solderability

80 / 100
70 / 100
70 / 100
65 / 100

Polishability

55 / 100
45 / 100
40 / 100
40 / 100

Same in both: Weldability 95 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Carbon (primary production)

2 kg CO₂/kg
1.9 kg CO₂/kg
2 kg CO₂/kg
2 kg CO₂/kg

Embodied Water

40 L/kg4.8 gal/lb
40 L/kg4.8 gal/lb
40 L/kg4.8 gal/lb
30 L/kg3.6 gal/lb

Typical Recycled Content

30%
30%
40%
25%

Same in both: Embodied Energy (primary production) 25 MJ/kg10,748 BTU/lb

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

54 kN·m/kg
54 kN·m/kg
57 kN·m/kg
54 kN·m/kg

Specific Stiffness (E / density)

26.8 MN·m/kg
25.5 MN·m/kg
25.5 MN·m/kg
26.2 MN·m/kg

Modulus of Resilience

161 kJ/m³
132 kJ/m³
169 kJ/m³
152 kJ/m³

Thermal Diffusivity

13.8 mm²/s
13.8 mm²/s
13.6 mm²/s
13.6 mm²/s

Thermal Shock Resistance Index

8
9
10
8

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleA283A36Q235BS235JR

Manufacturing and finishing

CapabilityS235JRA283A36Q235B
Default conditionHRHRHRHR
Relative cost$ Budget$ Budget$ Budget$ Budget
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining and Sheet metal. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in S235JR and A283 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.