FabDigit

P20 vs 4130 and 2 more: properties

P20413043408620

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

700 MPa102 ksi
700 MPa102 ksi
950 MPa138 ksi
635 MPa92.1 ksi

Yield Strength (0.2% offset)

440 MPa63.8 ksi
440 MPa63.8 ksi
620 MPa89.9 ksi
385 MPa55.8 ksi

Elongation at Break

20%
22%
18%
28%

Reduction in Area

55%
50%
45%
60%

Compressive Strength

900 MPa131 ksi
480 MPa69.6 ksi
640 MPa92.8 ksi

Shear Strength

620 MPa89.9 ksi
440 MPa63.8 ksi
580 MPa84.1 ksi
390 MPa56.6 ksi

Fatigue Strength (Endurance Limit)

460 MPa66.7 ksi
330 MPa47.9 ksi
430 MPa62.4 ksi
295 MPa42.8 ksi

Fracture Toughness (K_IC)

65 MPa·√m59.2 ksi·√in
110 MPa·√m100 ksi·√in
95 MPa·√m86.5 ksi·√in
85 MPa·√m77.4 ksi·√in

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
55 J40.6 ft·lbf
30 J22.1 ft·lbf
90 J66.4 ft·lbf

Hardness, Brinell

200 HB
210 HB
285 HB
183 HB

Hardness, Rockwell B

93 HRB
95 HRB
100 HRB
90 HRB

Hardness, Rockwell C

31 HRC
29 HRC

Hardness, Vickers

315 HV
228 HV
300 HV

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Density

7.8 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,420°C2,588 °F
1,432°C2,610 °F
1,416°C2,581 °F
1,425°C2,597 °F

Liquidus Temperature

1,480°C2,696 °F
1,510°C2,750 °F
1,454°C2,649 °F
1,505°C2,741 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

32 W/m·K18.5 BTU/hr·ft·°F
42.7 W/m·K24.7 BTU/hr·ft·°F
44.5 W/m·K25.7 BTU/hr·ft·°F
46.6 W/m·K26.9 BTU/hr·ft·°F

Specific Heat Capacity

460 J/kg·K0.11 BTU/lb·°F
477 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.4 µm/m·K6.9 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
11.6 µm/m·K6.4 µin/in·°F

Latent Heat of Fusion

250 J/g107 BTU/lb
272 J/g117 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb

Max Service Temperature (continuous)

450°C842 °F
400°C752 °F
400°C752 °F
400°C752 °F

Min Service Temperature

-20°C-4 °F
-50°C-58 °F
-40°C-40 °F
-40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.23×10⁻⁷ Ω·m8.78 µΩ·in
2.48×10⁻⁷ Ω·m9.76 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in

Electrical Conductivity

7.7 % IACS
7 % IACS
8 % IACS

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.61 V
-0.62 V
-0.6 V

Corrosion Resistance

15 / 100
14 / 100
12 / 100
11 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

65 / 100
55 / 100
48 / 100
62 / 100

Machinability Rating (AISI 1212 = 100 %)

75%
60%
50%
65%

Weldability

50 / 100
65 / 100
33 / 100
60 / 100

Formability (cold)

30 / 100
45 / 100
35 / 100
55 / 100

Brazeability / Solderability

40 / 100
70 / 100
55 / 100
65 / 100

Polishability

55 / 100
60 / 100
70 / 100
70 / 100

Castability

45 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

32 MJ/kg13,758 BTU/lb
30 MJ/kg12,898 BTU/lb
32 MJ/kg13,758 BTU/lb
30 MJ/kg12,898 BTU/lb

Embodied Carbon (primary production)

2.2 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.1 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
45 L/kg5.4 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

40%
30%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

90 kN·m/kg
89 kN·m/kg
121 kN·m/kg
81 kN·m/kg

Specific Stiffness (E / density)

26.3 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

472 kJ/m³
472 kJ/m³
938 kJ/m³
362 kJ/m³

Thermal Diffusivity

8.9 mm²/s
11.4 mm²/s
11.9 mm²/s
12.5 mm²/s

Thermal Shock Resistance Index

9
12
17
12

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale413043408620P20

Manufacturing and finishing

CapabilityP20413043408620
Sheet metalYesYesYes
Default conditionAnnealedHRHRHR
Relative cost$$$$$ Specialty$$ Standard$$$ Premium$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in P20 and 4130 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.