FabDigit

M27 vs M4 and 2 more: properties

M27M435W250M19

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

200 GPa29 Msi
217 GPa31.5 Msi
195 GPa28.3 Msi
200 GPa29 Msi

Shear Modulus

78 GPa11.3 Msi
84 GPa12.2 Msi
76 GPa11 Msi
78 GPa11.3 Msi

Bulk Modulus

160 GPa23.2 Msi
165 GPa23.9 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi

Poisson's Ratio

0.29
0.28
0.3
0.29

Tensile Strength (Ultimate)

450 MPa65.3 ksi
880 MPa128 ksi
480 MPa69.6 ksi
460 MPa66.7 ksi

Yield Strength (0.2% offset)

315 MPa45.7 ksi
550 MPa79.8 ksi
360 MPa52.2 ksi
340 MPa49.3 ksi

Elongation at Break

28%
12%
12%
25%

Shear Strength

300 MPa43.5 ksi
600 MPa87 ksi
330 MPa47.9 ksi
320 MPa46.4 ksi

Fatigue Strength (Endurance Limit)

210 MPa30.5 ksi
210 MPa30.5 ksi
230 MPa33.4 ksi

Hardness, Rockwell B

84 HRB
82 HRB
72 HRB

Hardness, Vickers

170 HV
265 HV
190 HV
150 HV

Reduction in Area

25%
45%

Compressive Strength

1,600 MPa232 ksi
360 MPa52.2 ksi

Fracture Toughness (K_IC)

22 MPa·√m20 ksi·√in

Hardness, Brinell

250 HB
180 HB

Hardness, Rockwell C

24 HRC

Charpy V-Notch Impact (RT)

5 J3.7 ft·lbf

Physical

Density and transition temperatures.

Density

7.75 g/cm³0.28 lb/in³
7.97 g/cm³0.29 lb/in³
7.65 g/cm³0.28 lb/in³
7.65 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,500°C2,732 °F
1,250°C2,282 °F
1,490°C2,714 °F
1,480°C2,696 °F

Liquidus Temperature

1,520°C2,768 °F
1,420°C2,588 °F
1,510°C2,750 °F
1,520°C2,768 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

25 W/m·K14.4 BTU/hr·ft·°F
22 W/m·K12.7 BTU/hr·ft·°F
24 W/m·K13.9 BTU/hr·ft·°F
25 W/m·K14.4 BTU/hr·ft·°F

Specific Heat Capacity

480 J/kg·K0.11 BTU/lb·°F
420 J/kg·K0.1 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
480 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

11.8 µm/m·K6.6 µin/in·°F
11 µm/m·K6.1 µin/in·°F
11.5 µm/m·K6.4 µin/in·°F
11.5 µm/m·K6.4 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
250 J/g107 BTU/lb
260 J/g112 BTU/lb
260 J/g112 BTU/lb

Max Service Temperature (continuous)

200°C392 °F
400°C752 °F
180°C356 °F
200°C392 °F

Same in both: Min Service Temperature -60°C-76 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

3.8 % IACS
2.9 % IACS
3.1 % IACS
3.3 % IACS

Electrical Resistivity

4.5×10⁻⁷ Ω·m17.7 µΩ·in
6×10⁻⁷ Ω·m23.6 µΩ·in
5.5×10⁻⁷ Ω·m21.7 µΩ·in
5.2×10⁻⁷ Ω·m20.5 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.58 V
-0.6 V

Corrosion Resistance

14 / 100
18 / 100
18 / 100
15 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

45 / 100
25 / 100
45 / 100
45 / 100

Machinability Rating (AISI 1212 = 100 %)

50%
25%
45%
45%

Weldability

55 / 100
15 / 100
35 / 100
50 / 100

Formability (cold)

60 / 100
12 / 100
45 / 100
65 / 100

Brazeability / Solderability

50 / 100
45 / 100
30 / 100
50 / 100

Polishability

45 / 100
50 / 100
40 / 100
50 / 100

Castability

20 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

34 MJ/kg14,617 BTU/lb
58 MJ/kg24,936 BTU/lb
32 MJ/kg13,758 BTU/lb
32 MJ/kg13,758 BTU/lb

Embodied Carbon (primary production)

2.5 kg CO₂/kg
4.2 kg CO₂/kg
2.4 kg CO₂/kg
2.4 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
110 L/kg13.2 gal/lb
45 L/kg5.4 gal/lb
55 L/kg6.6 gal/lb

Typical Recycled Content

25%
35%
15%
25%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

58 kN·m/kg
110 kN·m/kg
63 kN·m/kg
60 kN·m/kg

Specific Stiffness (E / density)

25.8 MN·m/kg
27.2 MN·m/kg
25.5 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

248 kJ/m³
697 kJ/m³
332 kJ/m³
289 kJ/m³

Thermal Diffusivity

6.7 mm²/s
6.6 mm²/s
6.7 mm²/s
6.8 mm²/s

Thermal Shock Resistance Index

5
8
5
5

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleM435W250M19M27

Manufacturing and finishing

CapabilityM27M435W250M19
CNC machiningYes
Sheet metalYesYes
Default conditionAnnealedFinal AnnealedAnnealed
Relative cost$ Budget$$$$$ Specialty$$ Standard$$ Standard
Min. machined wall0.8 mm
Best machined surfaceRa 1.6 µm
AlCrNYes
AlTiNYes
Black OxideYesYesYes
CVD Al2O3Yes
CVD TiCNYes
CVD TiNYes
CerakoteYesYesYes
Chrome PlatingYesYesYes
CrNYes
DLCYes
E-CoatingYesYesYes
HVOF CoatingYes
Hot-Dip GalvanizingYesYesYes
MoS2Yes
Multilayer CVDYes
Nickel PlatingYesYesYes
PTFE CoatingYesYesYes
PaintingYesYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in M27 and M4 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.