FabDigit

L6 vs A2 and 2 more: properties

L6A2A3O1

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

207 GPa30 Msi
203 GPa29.4 Msi
203 GPa29.4 Msi
205 GPa29.7 Msi

Shear Modulus

80 GPa11.6 Msi
78 GPa11.3 Msi
79 GPa11.5 Msi
79 GPa11.5 Msi

Poisson's Ratio

0.29
0.28
0.29
0.29

Tensile Strength (Ultimate)

730 MPa106 ksi
740 MPa107 ksi
760 MPa110 ksi
690 MPa100 ksi

Yield Strength (0.2% offset)

420 MPa60.9 ksi
470 MPa68.2 ksi
430 MPa62.4 ksi
400 MPa58 ksi

Elongation at Break

22%
22%
20%
25%

Reduction in Area

45%
45%
35%
45%

Compressive Strength

430 MPa62.4 ksi
500 MPa72.5 ksi
900 MPa131 ksi
420 MPa60.9 ksi

Shear Strength

440 MPa63.8 ksi
450 MPa65.3 ksi
460 MPa66.7 ksi
420 MPa60.9 ksi

Fatigue Strength (Endurance Limit)

330 MPa47.9 ksi
330 MPa47.9 ksi
320 MPa46.4 ksi

Charpy V-Notch Impact (RT)

40 J29.5 ft·lbf
30 J22.1 ft·lbf
25 J18.4 ft·lbf
30 J22.1 ft·lbf

Hardness, Brinell

197 HB
217 HB
217 HB
200 HB

Hardness, Rockwell B

92 HRB
96 HRB
96 HRB
94 HRB

Hardness, Vickers

207 HV
230 HV
228 HV
210 HV

Hardness, Rockwell C

19 HRC

Same in both: Bulk Modulus 160 GPa23.2 Msi

Physical

Density and transition temperatures.

Density

7.87 g/cm³0.28 lb/in³
7.86 g/cm³0.28 lb/in³
7.86 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,420°C2,588 °F
1,420°C2,588 °F
1,420°C2,588 °F
1,400°C2,552 °F

Liquidus Temperature

1,480°C2,696 °F
1,465°C2,669 °F
1,470°C2,678 °F
1,460°C2,660 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

38 W/m·K22 BTU/hr·ft·°F
26 W/m·K15 BTU/hr·ft·°F
24 W/m·K13.9 BTU/hr·ft·°F
35 W/m·K20.2 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

12.5 µm/m·K6.9 µin/in·°F
10.7 µm/m·K5.9 µin/in·°F
10.7 µm/m·K5.9 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F

Max Service Temperature (continuous)

400°C752 °F
425°C797 °F
200°C392 °F
400°C752 °F

Min Service Temperature

-50°C-58 °F
-30°C-22 °F
-30°C-22 °F
-30°C-22 °F

Same in both: Specific Heat Capacity 460 J/kg·K0.11 BTU/lb·°F · Latent Heat of Fusion 250 J/g107 BTU/lb

Electrical

Conductivity and insulation.

Electrical Conductivity

7 % IACS
2.7 % IACS
2.7 % IACS
7 % IACS

Electrical Resistivity

2.5×10⁻⁷ Ω·m9.84 µΩ·in
6.5×10⁻⁷ Ω·m25.6 µΩ·in
6.5×10⁻⁷ Ω·m25.6 µΩ·in
2.5×10⁻⁷ Ω·m9.84 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.6 V
-0.6 V

Corrosion Resistance

11 / 100
20 / 100
16 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
45 / 100
38 / 100
45 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
60%
42%
42%

Weldability

20 / 100
20 / 100
15 / 100
20 / 100

Formability (cold)

30 / 100
35 / 100
20 / 100
35 / 100

Castability

30 / 100
20 / 100
25 / 100

Brazeability / Solderability

40 / 100
40 / 100
35 / 100
45 / 100

Polishability

65 / 100
70 / 100
70 / 100
80 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

33 MJ/kg14,187 BTU/lb
36 MJ/kg15,477 BTU/lb
36 MJ/kg15,477 BTU/lb
32 MJ/kg13,758 BTU/lb

Embodied Carbon (primary production)

2.4 kg CO₂/kg
2.6 kg CO₂/kg
2.6 kg CO₂/kg
2.4 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
65 L/kg7.8 gal/lb
60 L/kg7.2 gal/lb
55 L/kg6.6 gal/lb

Typical Recycled Content

30%
35%
30%
40%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

93 kN·m/kg
94 kN·m/kg
97 kN·m/kg
88 kN·m/kg

Specific Stiffness (E / density)

26.3 MN·m/kg
25.8 MN·m/kg
25.8 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

426 kJ/m³
544 kJ/m³
455 kJ/m³
390 kJ/m³

Thermal Diffusivity

10.5 mm²/s
7.2 mm²/s
6.6 mm²/s
9.7 mm²/s

Thermal Shock Resistance Index

11
9
8
10

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleA2A3O1L6

Manufacturing and finishing

CapabilityL6A2A3O1
CNC machiningYesYesYes
Default conditionAnnealedAnnealed
Relative cost$$$ Premium$$$ Premium$$$ Premium$$$$ High
Min. machined wall0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µm
AlCrNYesYesYes
AlTiNYesYesYes
Black OxideYesYesYes
CVD Al2O3YesYesYes
CVD TiCNYesYesYes
CVD TiNYesYesYes
CerakoteYesYesYes
Chrome PlatingYesYesYes
CrNYesYesYes
DLCYesYesYes
E-CoatingYesYesYes
HVOF CoatingYesYesYes
Hot-Dip GalvanizingYesYesYes
MoS2YesYesYes
Multilayer CVDYesYesYes
Nickel PlatingYesYesYes
PTFE CoatingYesYesYes
PaintingYesYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in L6 and A2 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.