FabDigit

HSLA vs 4140 and 2 more: properties

HSLA414041504340

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

490 MPa71.1 ksi
690 MPa100 ksi
860 MPa125 ksi
950 MPa138 ksi

Yield Strength (0.2% offset)

345 MPa50 ksi
480 MPa69.6 ksi
520 MPa75.4 ksi
620 MPa89.9 ksi

Elongation at Break

21%
22%
16%
18%

Reduction in Area

50%
50%
40%
45%

Compressive Strength

345 MPa50 ksi
480 MPa69.6 ksi
640 MPa92.8 ksi

Shear Strength

300 MPa43.5 ksi
420 MPa60.9 ksi
560 MPa81.2 ksi
580 MPa84.1 ksi

Fatigue Strength (Endurance Limit)

240 MPa34.8 ksi
345 MPa50 ksi
390 MPa56.6 ksi
430 MPa62.4 ksi

Fracture Toughness (K_IC)

90 MPa·√m81.9 ksi·√in
110 MPa·√m100 ksi·√in
95 MPa·√m86.5 ksi·√in

Charpy V-Notch Impact (RT)

40 J29.5 ft·lbf
40 J29.5 ft·lbf
25 J18.4 ft·lbf
30 J22.1 ft·lbf

Hardness, Brinell

150 HB
210 HB
235 HB
285 HB

Hardness, Rockwell B

80 HRB
94 HRB
100 HRB

Hardness, Vickers

158 HV
220 HV
245 HV
300 HV

Hardness, Rockwell C

21 HRC
29 HRC

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,425°C2,597 °F
1,416°C2,581 °F
1,416°C2,581 °F
1,416°C2,581 °F

Liquidus Temperature

1,510°C2,750 °F
1,483°C2,701 °F
1,490°C2,714 °F
1,454°C2,649 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

45 W/m·K26 BTU/hr·ft·°F
42.6 W/m·K24.6 BTU/hr·ft·°F
42.6 W/m·K24.6 BTU/hr·ft·°F
44.5 W/m·K25.7 BTU/hr·ft·°F

Specific Heat Capacity

470 J/kg·K0.11 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12 µm/m·K6.7 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
425°C797 °F
400°C752 °F
400°C752 °F

Same in both: Min Service Temperature -40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

9 % IACS
7.8 % IACS
7.8 % IACS
7 % IACS

Electrical Resistivity

1.9×10⁻⁷ Ω·m7.48 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.48×10⁻⁷ Ω·m9.76 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.61 V
-0.61 V
-0.6 V
-0.62 V

Corrosion Resistance

16 / 100
12 / 100
12 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

58 / 100
60 / 100
45 / 100
48 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
62%
50%
50%

Weldability

80 / 100
40 / 100
25 / 100
33 / 100

Formability (cold)

60 / 100
40 / 100
25 / 100
35 / 100

Castability

30 / 100
35 / 100
45 / 100

Brazeability / Solderability

60 / 100
55 / 100
55 / 100
55 / 100

Polishability

50 / 100
60 / 100
60 / 100
70 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

25 MJ/kg10,748 BTU/lb
32 MJ/kg13,758 BTU/lb
31 MJ/kg13,328 BTU/lb
32 MJ/kg13,758 BTU/lb

Embodied Carbon (primary production)

2 kg CO₂/kg
2.2 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg

Embodied Water

45 L/kg5.4 gal/lb
55 L/kg6.6 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb

Same in both: Typical Recycled Content 30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

62 kN·m/kg
88 kN·m/kg
110 kN·m/kg
121 kN·m/kg

Modulus of Resilience

290 kJ/m³
562 kJ/m³
660 kJ/m³
938 kJ/m³

Thermal Diffusivity

12.2 mm²/s
11.5 mm²/s
11.5 mm²/s
11.9 mm²/s

Thermal Shock Resistance Index

9
12
15
17

Same in both: Specific Stiffness (E / density) 26.1 MN·m/kg

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale414041504340HSLA

Manufacturing and finishing

CapabilityHSLA414041504340
Casting & forgingYes
Default conditionHRHRHRHR
Relative cost$$ Standard$$ Standard$$$ Premium$$$ Premium
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining and Sheet metal. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in HSLA and 4140 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.