FabDigit

H13 vs H21 and 2 more: properties

H13H215CrMnMo5CrNiMo

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Poisson's Ratio

0.3
0.29
0.29
0.3

Tensile Strength (Ultimate)

760 MPa110 ksi
900 MPa131 ksi
780 MPa113 ksi
760 MPa110 ksi

Yield Strength (0.2% offset)

520 MPa75.4 ksi
620 MPa89.9 ksi
500 MPa72.5 ksi
450 MPa65.3 ksi

Elongation at Break

25%
18%
18%
18%

Reduction in Area

50%
40%
40%
45%

Compressive Strength

550 MPa79.8 ksi
650 MPa94.3 ksi
520 MPa75.4 ksi

Shear Strength

480 MPa69.6 ksi
550 MPa79.8 ksi
470 MPa68.2 ksi

Fatigue Strength (Endurance Limit)

360 MPa52.2 ksi
400 MPa58 ksi
350 MPa50.8 ksi

Charpy V-Notch Impact (RT)

40 J29.5 ft·lbf
25 J18.4 ft·lbf
45 J33.2 ft·lbf
35 J25.8 ft·lbf

Hardness, Brinell

205 HB
220 HB
220 HB
220 HB

Hardness, Rockwell B

95 HRB
97 HRB
97 HRB

Hardness, Vickers

215 HV
230 HV
230 HV
230 HV

Fracture Toughness (K_IC)

55 MPa·√m50.1 ksi·√in
80 MPa·√m72.8 ksi·√in
65 MPa·√m59.2 ksi·√in

Hardness, Rockwell C

19 HRC
18 HRC

Same in both: Elastic (Young's) Modulus 210 GPa30.5 Msi · Shear Modulus 81 GPa11.7 Msi · Bulk Modulus 160 GPa23.2 Msi

Physical

Density and transition temperatures.

Density

7.8 g/cm³0.28 lb/in³
8.28 g/cm³0.3 lb/in³
7.8 g/cm³0.28 lb/in³
7.83 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,425°C2,597 °F
1,420°C2,588 °F
1,420°C2,588 °F
1,420°C2,588 °F

Liquidus Temperature

1,480°C2,696 °F
1,480°C2,696 °F
1,470°C2,678 °F
1,480°C2,696 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

24.5 W/m·K14.2 BTU/hr·ft·°F
27 W/m·K15.6 BTU/hr·ft·°F
34 W/m·K19.6 BTU/hr·ft·°F
33 W/m·K19.1 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

10.9 µm/m·K6.1 µin/in·°F
11.8 µm/m·K6.6 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
12.5 µm/m·K6.9 µin/in·°F

Latent Heat of Fusion

250 J/g107 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
450°C842 °F
400°C752 °F
300°C572 °F

Min Service Temperature

-30°C-22 °F
-20°C-4 °F
-20°C-4 °F
-30°C-22 °F

Same in both: Specific Heat Capacity 460 J/kg·K0.11 BTU/lb·°F

Electrical

Conductivity and insulation.

Electrical Conductivity

3.3 % IACS
3.1 % IACS
7.2 % IACS

Electrical Resistivity

5.2×10⁻⁷ Ω·m20.5 µΩ·in
5.5×10⁻⁷ Ω·m21.7 µΩ·in
2.4×10⁻⁷ Ω·m9.45 µΩ·in
2.6×10⁻⁷ Ω·m10.2 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.58 V

Corrosion Resistance

22 / 100
15 / 100
12 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

45 / 100
40 / 100
55 / 100
55 / 100

Machinability Rating (AISI 1212 = 100 %)

50%
45%
55%
55%

Weldability

35 / 100
35 / 100
35 / 100
30 / 100

Formability (cold)

20 / 100
20 / 100
30 / 100
25 / 100

Brazeability / Solderability

30 / 100
40 / 100
35 / 100

Polishability

78 / 100
65 / 100
55 / 100
55 / 100

Castability

30 / 100
25 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

34 MJ/kg14,617 BTU/lb
42 MJ/kg18,057 BTU/lb
34 MJ/kg14,617 BTU/lb
32 MJ/kg13,758 BTU/lb

Embodied Carbon (primary production)

2.6 kg CO₂/kg
3 kg CO₂/kg
2.6 kg CO₂/kg
2.4 kg CO₂/kg

Embodied Water

75 L/kg9 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

45%
45%
45%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

97 kN·m/kg
109 kN·m/kg
100 kN·m/kg
97 kN·m/kg

Specific Stiffness (E / density)

26.9 MN·m/kg
25.4 MN·m/kg
26.9 MN·m/kg
26.8 MN·m/kg

Modulus of Resilience

644 kJ/m³
915 kJ/m³
595 kJ/m³
482 kJ/m³

Thermal Diffusivity

6.8 mm²/s
7.1 mm²/s
9.5 mm²/s
9.2 mm²/s

Thermal Shock Resistance Index

8
10
10
10

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleH13H215CrMnMo5CrNiMo

Manufacturing and finishing

CapabilityH13H215CrMnMo5CrNiMo
CNC machiningYesYes
3D printingYes
Default conditionAnnealedAnnealed
Relative cost$$$$ High$$ Standard$ Budget$$ Standard
Min. machined wall0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µm
AlCrNYesYes
AlTiNYesYes
Black OxideYesYes
CVD Al2O3YesYes
CVD TiCNYesYes
CVD TiNYesYes
CerakoteYesYes
Chrome PlatingYesYes
CrNYesYes
DLCYesYes
E-CoatingYesYes
HVOF CoatingYesYes
Hot-Dip GalvanizingYesYes
MoS2YesYes
Multilayer CVDYesYes
Nickel PlatingYesYes
PTFE CoatingYesYes
PaintingYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in H13 and H21 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.