Elastic (Young's) Modulus

186 GPa27 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi

Shear Modulus

71 GPa10.3 Msi
80 GPa11.6 Msi
80 GPa11.6 Msi
80 GPa11.6 Msi

Bulk Modulus

158 GPa22.9 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi

Poisson's Ratio

0.3
0.29
0.29
0.29

Tensile Strength (Ultimate)

1,050 MPa152 ksi
690 MPa100 ksi
860 MPa125 ksi
950 MPa138 ksi

Yield Strength (0.2% offset)

850 MPa123 ksi
480 MPa69.6 ksi
520 MPa75.4 ksi
620 MPa89.9 ksi

Elongation at Break

13%
22%
16%
18%

Reduction in Area

58%
50%
40%
45%

Compressive Strength

870 MPa126 ksi
480 MPa69.6 ksi
640 MPa92.8 ksi

Shear Strength

645 MPa93.5 ksi
420 MPa60.9 ksi
560 MPa81.2 ksi
580 MPa84.1 ksi

Fatigue Strength (Endurance Limit)

460 MPa66.7 ksi
345 MPa50 ksi
390 MPa56.6 ksi
430 MPa62.4 ksi

Fracture Toughness (K_IC)

130 MPa·√m118 ksi·√in
110 MPa·√m100 ksi·√in
95 MPa·√m86.5 ksi·√in

Charpy V-Notch Impact (RT)

105 J77.4 ft·lbf
40 J29.5 ft·lbf
25 J18.4 ft·lbf
30 J22.1 ft·lbf

Hardness, Brinell

310 HB
210 HB
235 HB
285 HB

Hardness, Rockwell C

32 HRC
21 HRC
29 HRC

Hardness, Vickers

320 HV
220 HV
245 HV
300 HV

Hardness, Rockwell B

94 HRB
100 HRB

Physical

Density and transition temperatures.

Density

8 g/cm³0.29 lb/in³
7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,413°C2,575 °F
1,416°C2,581 °F
1,416°C2,581 °F
1,416°C2,581 °F

Liquidus Temperature

1,440°C2,624 °F
1,483°C2,701 °F
1,490°C2,714 °F
1,454°C2,649 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

19.5 W/m·K11.3 BTU/hr·ft·°F
42.6 W/m·K24.6 BTU/hr·ft·°F
42.6 W/m·K24.6 BTU/hr·ft·°F
44.5 W/m·K25.7 BTU/hr·ft·°F

Specific Heat Capacity

452 J/kg·K0.11 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

10.1 µm/m·K5.6 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
425°C797 °F
400°C752 °F
400°C752 °F

Min Service Temperature

-196°C-321 °F
-40°C-40 °F
-40°C-40 °F
-40°C-40 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

2.9 % IACS
7.8 % IACS
7.8 % IACS
7 % IACS

Electrical Resistivity

6×10⁻⁷ Ω·m23.6 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.48×10⁻⁷ Ω·m9.76 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.61 V
-0.6 V
-0.62 V

Corrosion Resistance

22 / 100
12 / 100
12 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

42 / 100
60 / 100
45 / 100
48 / 100

Machinability Rating (AISI 1212 = 100 %)

42%
62%
50%
50%

Weldability

80 / 100
40 / 100
25 / 100
33 / 100

Formability (cold)

55 / 100
40 / 100
25 / 100
35 / 100

Castability

42 / 100
35 / 100
45 / 100

Brazeability / Solderability

50 / 100
55 / 100
55 / 100
55 / 100

Polishability

78 / 100
60 / 100
60 / 100
70 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

105 MJ/kg45,142 BTU/lb
32 MJ/kg13,758 BTU/lb
31 MJ/kg13,328 BTU/lb
32 MJ/kg13,758 BTU/lb

Embodied Carbon (primary production)

7 kg CO₂/kg
2.2 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg

Embodied Water

200 L/kg24 gal/lb
55 L/kg6.6 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

20%
30%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

131 kN·m/kg
88 kN·m/kg
110 kN·m/kg
121 kN·m/kg

Specific Stiffness (E / density)

23.3 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

1,942 kJ/m³
562 kJ/m³
660 kJ/m³
938 kJ/m³

Thermal Diffusivity

5.4 mm²/s
11.5 mm²/s
11.5 mm²/s
11.9 mm²/s

Thermal Shock Resistance Index

11
12
15
17

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale414041504340C300

Manufacturing and finishing

CapabilityC300414041504340
Casting & forgingYes
Default conditionHRHRHRHR
Relative cost$$$$$ Specialty$$ Standard$$$ Premium$$$ Premium
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining and Sheet metal. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.