FabDigit

A232 vs AR400 and 2 more: properties

A232AR400AR500A514

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

207 GPa30 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi

Shear Modulus

79.3 GPa11.5 Msi
80 GPa11.6 Msi
80 GPa11.6 Msi
80 GPa11.6 Msi

Tensile Strength (Ultimate)

1,750 MPa254 ksi
1,250 MPa181 ksi
1,650 MPa239 ksi
800 MPa116 ksi

Yield Strength (0.2% offset)

1,550 MPa225 ksi
1,050 MPa152 ksi
1,350 MPa196 ksi
760 MPa110 ksi

Elongation at Break

8%
11%
9%
19%

Reduction in Area

40%
40%
30%
50%

Shear Strength

1,050 MPa152 ksi
780 MPa113 ksi
1,000 MPa145 ksi
480 MPa69.6 ksi

Fatigue Strength (Endurance Limit)

720 MPa104 ksi
520 MPa75.4 ksi
700 MPa102 ksi
380 MPa55.1 ksi

Fracture Toughness (K_IC)

45 MPa·√m41 ksi·√in
70 MPa·√m63.7 ksi·√in
50 MPa·√m45.5 ksi·√in
120 MPa·√m109 ksi·√in

Charpy V-Notch Impact (RT)

14 J10.3 ft·lbf
30 J22.1 ft·lbf
35 J25.8 ft·lbf
75 J55.3 ft·lbf

Hardness, Brinell

495 HB
400 HB
500 HB
250 HB

Hardness, Rockwell C

50 HRC
43 HRC
50 HRC
24 HRC

Hardness, Vickers

520 HV
420 HV
525 HV
262 HV

Compressive Strength

1,100 MPa160 ksi
1,400 MPa203 ksi
760 MPa110 ksi

Hardness, Rockwell B

100 HRB

Same in both: Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,420°C2,588 °F
1,420°C2,588 °F
1,420°C2,588 °F
1,425°C2,597 °F

Liquidus Temperature

1,490°C2,714 °F
1,500°C2,732 °F
1,500°C2,732 °F
1,510°C2,750 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

46 W/m·K26.6 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F
40 W/m·K23.1 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F

Specific Heat Capacity

475 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.2 µm/m·K6.8 µin/in·°F
12 µm/m·K6.7 µin/in·°F
12 µm/m·K6.7 µin/in·°F
12 µm/m·K6.7 µin/in·°F

Latent Heat of Fusion

260 J/g112 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

230°C446 °F
250°C482 °F
250°C482 °F
400°C752 °F

Min Service Temperature

-40°C-40 °F
-20°C-4 °F
-40°C-40 °F
-45°C-49 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

7.5 % IACS
8 % IACS
7.5 % IACS
7 % IACS

Electrical Resistivity

2.3×10⁻⁷ Ω·m9.06 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.3×10⁻⁷ Ω·m9.06 µΩ·in
2.4×10⁻⁷ Ω·m9.45 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.62 V
-0.6 V

Corrosion Resistance

12 / 100
12 / 100
13 / 100
16 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

20 / 100
22 / 100
12 / 100
38 / 100

Machinability Rating (AISI 1212 = 100 %)

20%
20%
10%
40%

Weldability

20 / 100
55 / 100
45 / 100
55 / 100

Formability (cold)

25 / 100
25 / 100
15 / 100
30 / 100

Brazeability / Solderability

30 / 100
20 / 100
40 / 100

Polishability

65 / 100
55 / 100
55 / 100
50 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

31 MJ/kg13,328 BTU/lb
28 MJ/kg12,038 BTU/lb
30 MJ/kg12,898 BTU/lb
31 MJ/kg13,328 BTU/lb

Embodied Carbon (primary production)

2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.4 kg CO₂/kg

Embodied Water

55 L/kg6.6 gal/lb
45 L/kg5.4 gal/lb
55 L/kg6.6 gal/lb
45 L/kg5.4 gal/lb

Typical Recycled Content

25%
25%
25%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

223 kN·m/kg
159 kN·m/kg
210 kN·m/kg
102 kN·m/kg

Specific Stiffness (E / density)

26.4 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

5,803 kJ/m³
2,689 kJ/m³
4,445 kJ/m³
1,409 kJ/m³

Thermal Diffusivity

12.3 mm²/s
11.4 mm²/s
10.8 mm²/s
11.4 mm²/s

Thermal Shock Resistance Index

32
21
27
14

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleAR400AR500A514A232

Manufacturing and finishing

CapabilityA232AR400AR500A514
CNC machiningYesYesYes
Sheet metalYesYesYes
Default conditionQ&TQ&TQ&T
Relative cost$$ Standard$$$ Premium$$$$ High$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µm
AlCrNYesYesYes
AlTiNYesYesYes
Black OxideYesYesYes
CVD Al2O3YesYesYes
CVD TiCNYesYesYes
CVD TiNYesYesYes
CerakoteYesYesYes
Chrome PlatingYesYesYes
CrNYesYesYes
DLCYesYesYes
E-CoatingYesYesYes
HVOF CoatingYesYesYes
Hot-Dip GalvanizingYesYesYes
MoS2YesYesYes
Multilayer CVDYesYesYes
Nickel PlatingYesYesYes
PTFE CoatingYesYesYes
PaintingYesYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in A232 and AR400 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.