Tensile Strength (Ultimate)

520 MPa75.4 ksi
1,250 MPa181 ksi
1,650 MPa239 ksi
800 MPa116 ksi

Yield Strength (0.2% offset)

355 MPa51.5 ksi
1,050 MPa152 ksi
1,350 MPa196 ksi
760 MPa110 ksi

Elongation at Break

26%
11%
9%
19%

Reduction in Area

58%
40%
30%
50%

Compressive Strength

355 MPa51.5 ksi
1,100 MPa160 ksi
1,400 MPa203 ksi
760 MPa110 ksi

Shear Strength

330 MPa47.9 ksi
780 MPa113 ksi
1,000 MPa145 ksi
480 MPa69.6 ksi

Fatigue Strength (Endurance Limit)

250 MPa36.3 ksi
520 MPa75.4 ksi
700 MPa102 ksi
380 MPa55.1 ksi

Fracture Toughness (K_IC)

120 MPa·√m109 ksi·√in
70 MPa·√m63.7 ksi·√in
50 MPa·√m45.5 ksi·√in
120 MPa·√m109 ksi·√in

Charpy V-Notch Impact (RT)

150 J111 ft·lbf
30 J22.1 ft·lbf
35 J25.8 ft·lbf
75 J55.3 ft·lbf

Hardness, Brinell

160 HB
400 HB
500 HB
250 HB

Hardness, Rockwell B

84 HRB
—
—
100 HRB

Hardness, Rockwell C

—
43 HRC
50 HRC
24 HRC

Hardness, Vickers

—
420 HV
525 HV
262 HV

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,450°C2,642 °F
1,420°C2,588 °F
1,420°C2,588 °F
1,425°C2,597 °F

Liquidus Temperature

1,505°C2,741 °F
1,500°C2,732 °F
1,500°C2,732 °F
1,510°C2,750 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

40 W/m·K23.1 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F
40 W/m·K23.1 BTU/hr·ft·°F
42 W/m·K24.3 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

11.7 µm/m·K6.5 µin/in·°F
12 µm/m·K6.7 µin/in·°F
12 µm/m·K6.7 µin/in·°F
12 µm/m·K6.7 µin/in·°F

Latent Heat of Fusion

250 J/g107 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
250°C482 °F
250°C482 °F
400°C752 °F

Min Service Temperature

-46°C-51 °F
-20°C-4 °F
-40°C-40 °F
-45°C-49 °F

Same in both: Specific Heat Capacity 470 J/kg·K0.11 BTU/lb·°F

Electrical

Conductivity and insulation.

Electrical Conductivity

7.5 % IACS
8 % IACS
7.5 % IACS
7 % IACS

Electrical Resistivity

2.3×10⁻⁷ Ω·m9.06 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.3×10⁻⁷ Ω·m9.06 µΩ·in
2.4×10⁻⁷ Ω·m9.45 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.62 V
—
-0.62 V
-0.6 V

Corrosion Resistance

22 / 100
12 / 100
13 / 100
16 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

58 / 100
22 / 100
12 / 100
38 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
20%
10%
40%

Weldability

65 / 100
55 / 100
45 / 100
55 / 100

Formability (cold)

45 / 100
25 / 100
15 / 100
30 / 100

Brazeability / Solderability

50 / 100
20 / 100
—
40 / 100

Polishability

50 / 100
55 / 100
55 / 100
50 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

26 MJ/kg11,178 BTU/lb
28 MJ/kg12,038 BTU/lb
30 MJ/kg12,898 BTU/lb
31 MJ/kg13,328 BTU/lb

Embodied Carbon (primary production)

2.1 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.4 kg CO₂/kg

Embodied Water

40 L/kg4.8 gal/lb
45 L/kg5.4 gal/lb
55 L/kg6.6 gal/lb
45 L/kg5.4 gal/lb

Typical Recycled Content

30%
25%
25%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

66 kN·m/kg
159 kN·m/kg
210 kN·m/kg
102 kN·m/kg

Modulus of Resilience

307 kJ/m³
2,689 kJ/m³
4,445 kJ/m³
1,409 kJ/m³

Thermal Diffusivity

10.8 mm²/s
11.4 mm²/s
10.8 mm²/s
11.4 mm²/s

Thermal Shock Resistance Index

9
21
27
14

Same in both: Specific Stiffness (E / density) 26.1 MN·m/kg

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleAR400AR500A514A182 FR

Manufacturing and finishing

CapabilityA182 FRAR400AR500A514
CNC machining—YesYesYes
Sheet metal—YesYesYes
Default condition—Q&TQ&TQ&T
Relative cost$$ Standard$$$ Premium$$$$ High$$ Standard
Min. machined wall—0.8 mm0.8 mm0.8 mm
Best machined surface—Ra 1.6 µmRa 1.6 µmRa 1.6 µm
AlCrN—YesYesYes
AlTiN—YesYesYes
Black Oxide—YesYesYes
CVD Al2O3—YesYesYes
CVD TiCN—YesYesYes
CVD TiN—YesYesYes
Cerakote—YesYesYes
Chrome Plating—YesYesYes
CrN—YesYesYes
DLC—YesYesYes
E-Coating—YesYesYes
HVOF Coating—YesYesYes
Hot-Dip Galvanizing—YesYesYes
MoS2—YesYesYes
Multilayer CVD—YesYesYes
Nickel Plating—YesYesYes
PTFE Coating—YesYesYes
Painting—YesYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in A182 FR and AR400 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.