FabDigit

Steel 86B45 vs 10B21 vs 10B22 vs 15B35

Benchmark · 4 materials

Side-by-side benchmark of 4 steel grades.

86B45 vs 10B21 and 2 more: properties

86B4510B2110B2215B35

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

1,080 MPa157 ksi
430 MPa62.4 ksi
620 MPa89.9 ksi
730 MPa106 ksi

Yield Strength (0.2% offset)

950 MPa138 ksi
290 MPa42.1 ksi
525 MPa76.1 ksi
620 MPa89.9 ksi

Elongation at Break

16%
30%
13%
13%

Reduction in Area

50%
55%
48%
40%

Compressive Strength

960 MPa139 ksi
620 MPa89.9 ksi

Shear Strength

650 MPa94.3 ksi
275 MPa39.9 ksi
375 MPa54.4 ksi
440 MPa63.8 ksi

Fatigue Strength (Endurance Limit)

490 MPa71.1 ksi
200 MPa29 ksi
280 MPa40.6 ksi
330 MPa47.9 ksi

Fracture Toughness (K_IC)

80 MPa·√m72.8 ksi·√in
90 MPa·√m81.9 ksi·√in
75 MPa·√m68.3 ksi·√in

Charpy V-Notch Impact (RT)

45 J33.2 ft·lbf
65 J47.9 ft·lbf
45 J33.2 ft·lbf
25 J18.4 ft·lbf

Hardness, Brinell

320 HB
126 HB
180 HB
217 HB

Hardness, Rockwell C

34 HRC

Hardness, Vickers

336 HV

Hardness, Rockwell B

71 HRB
89 HRB
96 HRB

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,420°C2,588 °F
1,465°C2,669 °F
1,450°C2,642 °F
1,425°C2,597 °F

Liquidus Temperature

1,490°C2,714 °F
1,510°C2,750 °F
1,510°C2,750 °F
1,495°C2,723 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

42 W/m·K24.3 BTU/hr·ft·°F
51.9 W/m·K30 BTU/hr·ft·°F
49 W/m·K28.3 BTU/hr·ft·°F
46 W/m·K26.6 BTU/hr·ft·°F

Specific Heat Capacity

475 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.3 µm/m·K6.8 µin/in·°F
11.7 µm/m·K6.5 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F

Latent Heat of Fusion

260 J/g112 BTU/lb
247 J/g106 BTU/lb
250 J/g107 BTU/lb
247 J/g106 BTU/lb

Max Service Temperature (continuous)

400°C752 °F
400°C752 °F
350°C662 °F
350°C662 °F

Min Service Temperature

-40°C-40 °F
-30°C-22 °F
-30°C-22 °F
-30°C-22 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

7.8 % IACS
10.8 % IACS
10 % IACS
9.5 % IACS

Electrical Resistivity

2.2×10⁻⁷ Ω·m8.66 µΩ·in
1.6×10⁻⁷ Ω·m6.3 µΩ·in
1.7×10⁻⁷ Ω·m6.69 µΩ·in
1.8×10⁻⁷ Ω·m7.09 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.61 V
-0.61 V
-0.6 V
-0.61 V

Corrosion Resistance

11 / 100
10 / 100
10 / 100
10 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

42 / 100
62 / 100
55 / 100
55 / 100

Machinability Rating (AISI 1212 = 100 %)

45%
65%
65%
65%

Weldability

28 / 100
85 / 100
72 / 100
40 / 100

Formability (cold)

22 / 100
82 / 100
85 / 100
55 / 100

Brazeability / Solderability

50 / 100
70 / 100
65 / 100
60 / 100

Polishability

62 / 100
45 / 100
50 / 100
55 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

28 MJ/kg12,038 BTU/lb
25 MJ/kg10,748 BTU/lb
25 MJ/kg10,748 BTU/lb
25 MJ/kg10,748 BTU/lb

Embodied Carbon (primary production)

2.2 kg CO₂/kg
1.9 kg CO₂/kg
1.9 kg CO₂/kg
1.9 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
40 L/kg4.8 gal/lb
40 L/kg4.8 gal/lb
40 L/kg4.8 gal/lb

Same in both: Typical Recycled Content 30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

138 kN·m/kg
55 kN·m/kg
79 kN·m/kg
93 kN·m/kg

Modulus of Resilience

2,201 kJ/m³
205 kJ/m³
672 kJ/m³
938 kJ/m³

Thermal Diffusivity

11.3 mm²/s
14.1 mm²/s
13.3 mm²/s
12.3 mm²/s

Thermal Shock Resistance Index

18
9
12
14

Same in both: Specific Stiffness (E / density) 26.1 MN·m/kg

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale10B2110B2215B3586B45

Manufacturing and finishing

Capability86B4510B2110B2215B35
CNC machiningYes
Sheet metalYes
Default conditionHR
Relative cost$ Budget$ Budget$ Budget$ Budget
Min. machined wall0.8 mm
Best machined surfaceRa 1.6 µm
AlCrNYes
AlTiNYes
Black OxideYes
CVD Al2O3Yes
CVD TiCNYes
CVD TiNYes
CerakoteYes
Chrome PlatingYes
CrNYes
DLCYes
E-CoatingYes
HVOF CoatingYes
Hot-Dip GalvanizingYes
MoS2Yes
Multilayer CVDYes
Nickel PlatingYes
PTFE CoatingYes
PaintingYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 86B45 and 10B21 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.