FabDigit

5160 vs 4140 and 2 more: properties

5160414041505120

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Tensile Strength (Ultimate)

725 MPa105 ksi
690 MPa100 ksi
860 MPa125 ksi
470 MPa68.2 ksi

Yield Strength (0.2% offset)

275 MPa39.9 ksi
480 MPa69.6 ksi
520 MPa75.4 ksi
295 MPa42.8 ksi

Elongation at Break

17%
22%
16%
25%

Reduction in Area

31%
50%
40%
55%

Shear Strength

450 MPa65.3 ksi
420 MPa60.9 ksi
560 MPa81.2 ksi
300 MPa43.5 ksi

Fatigue Strength (Endurance Limit)

330 MPa47.9 ksi
345 MPa50 ksi
390 MPa56.6 ksi
235 MPa34.1 ksi

Charpy V-Notch Impact (RT)

25 J18.4 ft·lbf
40 J29.5 ft·lbf
25 J18.4 ft·lbf
60 J44.3 ft·lbf

Hardness, Brinell

197 HB
210 HB
235 HB
145 HB

Hardness, Rockwell B

92 HRB
94 HRB
78 HRB

Compressive Strength

480 MPa69.6 ksi
295 MPa42.8 ksi

Fracture Toughness (K_IC)

110 MPa·√m100 ksi·√in
90 MPa·√m81.9 ksi·√in

Hardness, Vickers

220 HV
245 HV
152 HV

Hardness, Rockwell C

21 HRC

Same in both: Elastic (Young's) Modulus 205 GPa29.7 Msi · Shear Modulus 80 GPa11.6 Msi · Bulk Modulus 160 GPa23.2 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,425°C2,597 °F
1,416°C2,581 °F
1,416°C2,581 °F
1,420°C2,588 °F

Liquidus Temperature

1,490°C2,714 °F
1,483°C2,701 °F
1,490°C2,714 °F
1,500°C2,732 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

46 W/m·K26.6 BTU/hr·ft·°F
42.6 W/m·K24.6 BTU/hr·ft·°F
42.6 W/m·K24.6 BTU/hr·ft·°F
46 W/m·K26.6 BTU/hr·ft·°F

Specific Heat Capacity

490 J/kg·K0.12 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F
470 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

12.3 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F

Latent Heat of Fusion

250 J/g107 BTU/lb
250 J/g107 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb

Max Service Temperature (continuous)

250°C482 °F
425°C797 °F
400°C752 °F
350°C662 °F

Min Service Temperature

-40°C-40 °F
-40°C-40 °F
-40°C-40 °F
-30°C-22 °F

Electrical

Conductivity and insulation.

Same in both: Electrical Conductivity 7.8 % IACS · Electrical Resistivity 2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.61 V
-0.61 V
-0.6 V
-0.61 V

Corrosion Resistance

10 / 100
12 / 100
12 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
60 / 100
45 / 100
62 / 100

Machinability Rating (AISI 1212 = 100 %)

56%
62%
50%
65%

Weldability

25 / 100
40 / 100
25 / 100
60 / 100

Formability (cold)

45 / 100
40 / 100
25 / 100
58 / 100

Castability

40 / 100
35 / 100

Brazeability / Solderability

55 / 100
55 / 100
55 / 100
70 / 100

Polishability

70 / 100
60 / 100
60 / 100
55 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

30 MJ/kg12,898 BTU/lb
32 MJ/kg13,758 BTU/lb
31 MJ/kg13,328 BTU/lb
25 MJ/kg10,748 BTU/lb

Embodied Carbon (primary production)

2.2 kg CO₂/kg
2.2 kg CO₂/kg
2.3 kg CO₂/kg
1.9 kg CO₂/kg

Embodied Water

60 L/kg7.2 gal/lb
55 L/kg6.6 gal/lb
60 L/kg7.2 gal/lb
45 L/kg5.4 gal/lb

Typical Recycled Content

35%
30%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

92 kN·m/kg
88 kN·m/kg
110 kN·m/kg
60 kN·m/kg

Modulus of Resilience

184 kJ/m³
562 kJ/m³
660 kJ/m³
212 kJ/m³

Thermal Diffusivity

12 mm²/s
11.5 mm²/s
11.5 mm²/s
12.5 mm²/s

Thermal Shock Resistance Index

13
12
15
9

Same in both: Specific Stiffness (E / density) 26.1 MN·m/kg

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale4140415051605120

Manufacturing and finishing

Capability5160414041505120
Casting & forgingYes
Default conditionAnnealedHRHRHR
Relative cost$$$ Premium$$ Standard$$$ Premium$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µmRa 1.6 µm

Both are offered for CNC machining and Sheet metal. Both take the same 38 finishes: AlCrN, AlTiN, Black Oxide, CVD Al2O3, CVD TiCN, CVD TiN, Cerakote, Chrome Plating, Copper Plating, CrN, DLC, E-Coating and 26 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 5160 and 4140 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.