4Cr5MoSiVH13H215CrMnMo

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Bulk Modulus

168 GPa24.4 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi

Poisson's Ratio

0.3
0.3
0.29
0.29

Tensile Strength (Ultimate)

780 MPa113 ksi
760 MPa110 ksi
900 MPa131 ksi
780 MPa113 ksi

Yield Strength (0.2% offset)

500 MPa72.5 ksi
520 MPa75.4 ksi
620 MPa89.9 ksi
500 MPa72.5 ksi

Elongation at Break

22%
25%
18%
18%

Reduction in Area

50%
50%
40%
40%

Compressive Strength

520 MPa75.4 ksi
550 MPa79.8 ksi
650 MPa94.3 ksi
520 MPa75.4 ksi

Shear Strength

470 MPa68.2 ksi
480 MPa69.6 ksi
550 MPa79.8 ksi
470 MPa68.2 ksi

Fatigue Strength (Endurance Limit)

360 MPa52.2 ksi
360 MPa52.2 ksi
400 MPa58 ksi
350 MPa50.8 ksi

Charpy V-Notch Impact (RT)

60 J44.3 ft·lbf
40 J29.5 ft·lbf
25 J18.4 ft·lbf
45 J33.2 ft·lbf

Hardness, Brinell

210 HB
205 HB
220 HB
220 HB

Hardness, Rockwell B

95 HRB
95 HRB
97 HRB
97 HRB

Hardness, Vickers

220 HV
215 HV
230 HV
230 HV

Fracture Toughness (K_IC)

55 MPa·√m50.1 ksi·√in
80 MPa·√m72.8 ksi·√in

Hardness, Rockwell C

19 HRC
18 HRC

Same in both: Elastic (Young's) Modulus 210 GPa30.5 Msi · Shear Modulus 81 GPa11.7 Msi

Physical

Density and transition temperatures.

Density

7.8 g/cm³0.28 lb/in³
7.8 g/cm³0.28 lb/in³
8.28 g/cm³0.3 lb/in³
7.8 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,420°C2,588 °F
1,425°C2,597 °F
1,420°C2,588 °F
1,420°C2,588 °F

Liquidus Temperature

1,480°C2,696 °F
1,480°C2,696 °F
1,480°C2,696 °F
1,470°C2,678 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

24.5 W/m·K14.2 BTU/hr·ft·°F
24.5 W/m·K14.2 BTU/hr·ft·°F
27 W/m·K15.6 BTU/hr·ft·°F
34 W/m·K19.6 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

11.9 µm/m·K6.6 µin/in·°F
10.9 µm/m·K6.1 µin/in·°F
11.8 µm/m·K6.6 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F

Max Service Temperature (continuous)

400°C752 °F
400°C752 °F
450°C842 °F
400°C752 °F

Min Service Temperature

-20°C-4 °F
-30°C-22 °F
-20°C-4 °F
-20°C-4 °F

Same in both: Specific Heat Capacity 460 J/kg·K0.11 BTU/lb·°F · Latent Heat of Fusion 250 J/g107 BTU/lb

Electrical

Conductivity and insulation.

Electrical Conductivity

3.3 % IACS
3.3 % IACS
3.1 % IACS
7.2 % IACS

Electrical Resistivity

5.2×10⁻⁷ Ω·m20.5 µΩ·in
5.2×10⁻⁷ Ω·m20.5 µΩ·in
5.5×10⁻⁷ Ω·m21.7 µΩ·in
2.4×10⁻⁷ Ω·m9.45 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.55 V
-0.58 V

Corrosion Resistance

18 / 100
22 / 100
15 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
45 / 100
40 / 100
55 / 100

Machinability Rating (AISI 1212 = 100 %)

60%
50%
45%
55%

Formability (cold)

25 / 100
20 / 100
20 / 100
30 / 100

Castability

30 / 100
30 / 100
25 / 100

Brazeability / Solderability

40 / 100
30 / 100
40 / 100
35 / 100

Polishability

78 / 100
78 / 100
65 / 100
55 / 100

Same in both: Weldability 35 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

34 MJ/kg14,617 BTU/lb
34 MJ/kg14,617 BTU/lb
42 MJ/kg18,057 BTU/lb
34 MJ/kg14,617 BTU/lb

Embodied Carbon (primary production)

2.5 kg CO₂/kg
2.6 kg CO₂/kg
3 kg CO₂/kg
2.6 kg CO₂/kg

Embodied Water

70 L/kg8.4 gal/lb
75 L/kg9 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb

Same in both: Typical Recycled Content 45%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

100 kN·m/kg
97 kN·m/kg
109 kN·m/kg
100 kN·m/kg

Specific Stiffness (E / density)

26.9 MN·m/kg
26.9 MN·m/kg
25.4 MN·m/kg
26.9 MN·m/kg

Modulus of Resilience

595 kJ/m³
644 kJ/m³
915 kJ/m³
595 kJ/m³

Thermal Diffusivity

6.8 mm²/s
6.8 mm²/s
7.1 mm²/s
9.5 mm²/s

Thermal Shock Resistance Index

8
8
10
10

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleH13H215CrMnMo4Cr5MoSiV

Manufacturing and finishing

Capability4Cr5MoSiVH13H215CrMnMo
CNC machiningYesYes
3D printingYes
Default conditionAnnealedAnnealed
Relative cost$$ Standard$$$$ High$$ Standard$ Budget
Min. machined wall0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µm
AlCrNYesYes
AlTiNYesYes
Black OxideYesYes
CVD Al2O3YesYes
CVD TiCNYesYes
CVD TiNYesYes
CerakoteYesYes
Chrome PlatingYesYes
CrNYesYes
DLCYesYes
E-CoatingYesYes
HVOF CoatingYesYes
Hot-Dip GalvanizingYesYes
MoS2YesYes
Multilayer CVDYesYes
Nickel PlatingYesYes
PTFE CoatingYesYes
PaintingYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 4Cr5MoSiV and H13 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.