Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

190 GPa27.6 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi

Shear Modulus

73 GPa10.6 Msi
80 GPa11.6 Msi
80 GPa11.6 Msi
80 GPa11.6 Msi

Poisson's Ratio

0.3
0.29
0.29
0.29

Tensile Strength (Ultimate)

2,400 MPa348 ksi
700 MPa102 ksi
950 MPa138 ksi
635 MPa92.1 ksi

Yield Strength (0.2% offset)

2,300 MPa334 ksi
440 MPa63.8 ksi
620 MPa89.9 ksi
385 MPa55.8 ksi

Elongation at Break

7%
22%
18%
28%

Reduction in Area

35%
50%
45%
60%

Compressive Strength

2,400 MPa348 ksi
480 MPa69.6 ksi
640 MPa92.8 ksi

Shear Strength

1,400 MPa203 ksi
440 MPa63.8 ksi
580 MPa84.1 ksi
390 MPa56.6 ksi

Fatigue Strength (Endurance Limit)

800 MPa116 ksi
330 MPa47.9 ksi
430 MPa62.4 ksi
295 MPa42.8 ksi

Fracture Toughness (K_IC)

38 MPa·√m34.6 ksi·√in
110 MPa·√m100 ksi·√in
95 MPa·√m86.5 ksi·√in
85 MPa·√m77.4 ksi·√in

Charpy V-Notch Impact (RT)

14 J10.3 ft·lbf
55 J40.6 ft·lbf
30 J22.1 ft·lbf
90 J66.4 ft·lbf

Hardness, Rockwell C

57 HRC
29 HRC

Hardness, Vickers

660 HV
228 HV
300 HV

Hardness, Brinell

210 HB
285 HB
183 HB

Hardness, Rockwell B

95 HRB
100 HRB
90 HRB

Same in both: Bulk Modulus 160 GPa23.2 Msi

Physical

Density and transition temperatures.

Density

8.08 g/cm³0.29 lb/in³
7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³
7.85 g/cm³0.28 lb/in³

Melting Point (Solidus)

1,413°C2,575 °F
1,432°C2,610 °F
1,416°C2,581 °F
1,425°C2,597 °F

Liquidus Temperature

1,440°C2,624 °F
1,510°C2,750 °F
1,454°C2,649 °F
1,505°C2,741 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

15 W/m·K8.7 BTU/hr·ft·°F
42.7 W/m·K24.7 BTU/hr·ft·°F
44.5 W/m·K25.7 BTU/hr·ft·°F
46.6 W/m·K26.9 BTU/hr·ft·°F

Specific Heat Capacity

450 J/kg·K0.11 BTU/lb·°F
477 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

10.3 µm/m·K5.7 µin/in·°F
12.2 µm/m·K6.8 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
11.6 µm/m·K6.4 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
272 J/g117 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb

Min Service Temperature

-50°C-58 °F
-50°C-58 °F
-40°C-40 °F
-40°C-40 °F

Same in both: Max Service Temperature (continuous) 400°C752 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

2.7 % IACS
7.7 % IACS
7 % IACS
8 % IACS

Electrical Resistivity

6.5×10⁻⁷ Ω·m25.6 µΩ·in
2.23×10⁻⁷ Ω·m8.78 µΩ·in
2.48×10⁻⁷ Ω·m9.76 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.55 V
-0.61 V
-0.62 V
-0.6 V

Corrosion Resistance

25 / 100
14 / 100
12 / 100
11 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

18 / 100
55 / 100
48 / 100
62 / 100

Machinability Rating (AISI 1212 = 100 %)

15%
60%
50%
65%

Weldability

55 / 100
65 / 100
33 / 100
60 / 100

Formability (cold)

20 / 100
45 / 100
35 / 100
55 / 100

Castability

45 / 100
45 / 100

Brazeability / Solderability

40 / 100
70 / 100
55 / 100
65 / 100

Polishability

85 / 100
60 / 100
70 / 100
70 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

70 MJ/kg30,095 BTU/lb
30 MJ/kg12,898 BTU/lb
32 MJ/kg13,758 BTU/lb
30 MJ/kg12,898 BTU/lb

Embodied Carbon (primary production)

5.2 kg CO₂/kg
2.3 kg CO₂/kg
2.3 kg CO₂/kg
2.1 kg CO₂/kg

Embodied Water

110 L/kg13.2 gal/lb
45 L/kg5.4 gal/lb
60 L/kg7.2 gal/lb
60 L/kg7.2 gal/lb

Typical Recycled Content

20%
30%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

297 kN·m/kg
89 kN·m/kg
121 kN·m/kg
81 kN·m/kg

Specific Stiffness (E / density)

23.5 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

13,921 kJ/m³
472 kJ/m³
938 kJ/m³
362 kJ/m³

Thermal Diffusivity

4.1 mm²/s
11.4 mm²/s
11.9 mm²/s
12.5 mm²/s

Thermal Shock Resistance Index

18
12
17
12

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scale41304340862018Ni350

Manufacturing and finishing

Capability18Ni350413043408620
CNC machiningYesYesYes
Sheet metalYesYesYes
Default conditionHRHRHR
Relative cost$$$$ High$$ Standard$$$ Premium$$ Standard
Min. machined wall0.8 mm0.8 mm0.8 mm
Best machined surfaceRa 1.6 µmRa 1.6 µmRa 1.6 µm
AlCrNYesYesYes
AlTiNYesYesYes
Black OxideYesYesYes
CVD Al2O3YesYesYes
CVD TiCNYesYesYes
CVD TiNYesYesYes
CerakoteYesYesYes
Chrome PlatingYesYesYes
CrNYesYesYes
DLCYesYesYes
E-CoatingYesYesYes
HVOF CoatingYesYesYes
Hot-Dip GalvanizingYesYesYes
MoS2YesYesYes
Multilayer CVDYesYesYes
Nickel PlatingYesYesYes
PTFE CoatingYesYesYes
PaintingYesYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 18Ni350 and 4130 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.