18Kh2N4MASCM41543204620

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

210 GPa30.5 Msi
206 GPa29.9 Msi
205 GPa29.7 Msi
205 GPa29.7 Msi

Bulk Modulus

163 GPa23.6 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi
160 GPa23.2 Msi

Tensile Strength (Ultimate)

1,250 MPa181 ksi
640 MPa92.8 ksi
640 MPa92.8 ksi
570 MPa82.7 ksi

Yield Strength (0.2% offset)

980 MPa142 ksi
430 MPa62.4 ksi
415 MPa60.2 ksi
360 MPa52.2 ksi

Elongation at Break

13%
22%
22%
26%

Reduction in Area

55%
55%
50%
55%

Compressive Strength

1,000 MPa145 ksi
430 MPa62.4 ksi
—
—

Shear Strength

750 MPa109 ksi
400 MPa58 ksi
415 MPa60.2 ksi
380 MPa55.1 ksi

Fatigue Strength (Endurance Limit)

560 MPa81.2 ksi
290 MPa42.1 ksi
300 MPa43.5 ksi
260 MPa37.7 ksi

Fracture Toughness (K_IC)

80 MPa·√m72.8 ksi·√in
90 MPa·√m81.9 ksi·√in
—
—

Charpy V-Notch Impact (RT)

95 J70.1 ft·lbf
55 J40.6 ft·lbf
70 J51.6 ft·lbf
85 J62.7 ft·lbf

Hardness, Brinell

363 HB
180 HB
187 HB
163 HB

Hardness, Rockwell C

39 HRC
—
—
—

Hardness, Rockwell B

—
89 HRB
90 HRB
84 HRB

Hardness, Vickers

—
190 HV
—
—

Same in both: Shear Modulus 80 GPa11.6 Msi · Poisson's Ratio 0.29

Physical

Density and transition temperatures.

Melting Point (Solidus)

1,420°C2,588 °F
1,430°C2,606 °F
1,425°C2,597 °F
1,420°C2,588 °F

Liquidus Temperature

1,490°C2,714 °F
1,510°C2,750 °F
1,500°C2,732 °F
1,500°C2,732 °F

Same in both: Density 7.85 g/cm³0.28 lb/in³

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

33 W/m·K19.1 BTU/hr·ft·°F
44 W/m·K25.4 BTU/hr·ft·°F
44 W/m·K25.4 BTU/hr·ft·°F
46 W/m·K26.6 BTU/hr·ft·°F

Specific Heat Capacity

470 J/kg·K0.11 BTU/lb·°F
473 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F
475 J/kg·K0.11 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

11.5 µm/m·K6.4 µin/in·°F
12.3 µm/m·K6.8 µin/in·°F
11.7 µm/m·K6.5 µin/in·°F
11.9 µm/m·K6.6 µin/in·°F

Latent Heat of Fusion

270 J/g116 BTU/lb
250 J/g107 BTU/lb
270 J/g116 BTU/lb
250 J/g107 BTU/lb

Max Service Temperature (continuous)

200°C392 °F
400°C752 °F
350°C662 °F
400°C752 °F

Min Service Temperature

-70°C-94 °F
-50°C-58 °F
-60°C-76 °F
-50°C-58 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

3.5×10⁻⁷ Ω·m13.8 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in
2.2×10⁻⁷ Ω·m8.66 µΩ·in

Electrical Conductivity

—
7.8 % IACS
—
8 % IACS

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.6 V
-0.61 V
-0.6 V
-0.61 V

Corrosion Resistance

14 / 100
12 / 100
11 / 100
12 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

22 / 100
58 / 100
50 / 100
57 / 100

Machinability Rating (AISI 1212 = 100 %)

20%
60%
55%
65%

Weldability

22 / 100
55 / 100
40 / 100
65 / 100

Formability (cold)

18 / 100
60 / 100
45 / 100
58 / 100

Brazeability / Solderability

45 / 100
65 / 100
55 / 100
70 / 100

Polishability

70 / 100
60 / 100
60 / 100
55 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

36 MJ/kg15,477 BTU/lb
27 MJ/kg11,608 BTU/lb
31 MJ/kg13,328 BTU/lb
29 MJ/kg12,468 BTU/lb

Embodied Carbon (primary production)

2.7 kg CO₂/kg
2.1 kg CO₂/kg
2.3 kg CO₂/kg
2.2 kg CO₂/kg

Embodied Water

70 L/kg8.4 gal/lb
50 L/kg6 gal/lb
50 L/kg6 gal/lb
55 L/kg6.6 gal/lb

Typical Recycled Content

25%
30%
30%
30%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

159 kN·m/kg
82 kN·m/kg
82 kN·m/kg
73 kN·m/kg

Specific Stiffness (E / density)

26.8 MN·m/kg
26.2 MN·m/kg
26.1 MN·m/kg
26.1 MN·m/kg

Modulus of Resilience

2,287 kJ/m³
449 kJ/m³
420 kJ/m³
316 kJ/m³

Thermal Diffusivity

8.9 mm²/s
11.9 mm²/s
11.8 mm²/s
12.3 mm²/s

Thermal Shock Resistance Index

17
11
12
11

Strength versus weight

Yield strength against density for every steel grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

2005001,0002,0007.588.5Density (g/cm³)Yield strength (MPa) — log scaleSCM4154320462018Kh2N4MA

Manufacturing and finishing

Capability18Kh2N4MASCM41543204620
CNC machining—YesYesYes
Sheet metal—YesYesYes
Default condition—HRHRHR
Relative cost$$ Standard$$ Standard$$$ Premium$$ Standard
Min. machined wall—0.8 mm0.8 mm0.8 mm
Best machined surface—Ra 1.6 µmRa 1.6 µmRa 1.6 µm
AlCrN—YesYesYes
AlTiN—YesYesYes
Black Oxide—YesYesYes
CVD Al2O3—YesYesYes
CVD TiCN—YesYesYes
CVD TiN—YesYesYes
Cerakote—YesYesYes
Chrome Plating—YesYesYes
CrN—YesYesYes
DLC—YesYesYes
E-Coating—YesYesYes
HVOF Coating—YesYesYes
Hot-Dip Galvanizing—YesYesYes
MoS2—YesYesYes
Multilayer CVD—YesYesYes
Nickel Plating—YesYesYes
PTFE Coating—YesYesYes
Painting—YesYesYes

They share 9 finishes: Copper Plating, Electroless Nickel (EN), Epoxy Coating, Gold Plating, Hard Chrome Plating, Manganese Phosphate, Plasma Spray, Silver Plating, Zinc Phosphate.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 18Kh2N4MA and SCM415 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.