FabDigit

Vero vs PA6 and 2 more: properties

VeroPA6PA66PC-ABS

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

2.5 GPa0.36 Msi
3 GPa0.44 Msi
3 GPa0.44 Msi
2.4 GPa0.35 Msi

Poisson's Ratio

0.35
0.39
0.39
0.39

Tensile Strength (Ultimate)

57 MPa8.3 ksi
80 MPa11.6 ksi
82 MPa11.9 ksi
56 MPa8.1 ksi

Elongation at Break

17%
60%
40%
90%

Flexural Strength

90 MPa13.1 ksi
105 MPa15.2 ksi
105 MPa15.2 ksi
85 MPa12.3 ksi

Flexural Modulus

2.7 GPa0.39 Msi
2.8 GPa0.41 Msi
2.9 GPa0.42 Msi
2.3 GPa0.33 Msi

Izod Impact, Notched

25 J/m0.47 ft·lbf/in
55 J/m1 ft·lbf/in
50 J/m0.94 ft·lbf/in
500 J/m9.4 ft·lbf/in

Hardness, Shore D

84 Shore D
81 Shore D
81 Shore D
79 Shore D

Hardness, Rockwell M

74 HRM
82 HRM
85 HRM
68 HRM

Shear Modulus

1.1 GPa0.15 Msi
1.1 GPa0.16 Msi
0.87 GPa0.13 Msi

Bulk Modulus

5 GPa0.65 Msi
5 GPa0.65 Msi
4 GPa0.52 Msi

Yield Strength (0.2% offset)

75 MPa10.9 ksi
80 MPa11.6 ksi
55 MPa8 ksi

Compressive Strength

85 MPa12.3 ksi
95 MPa13.8 ksi
65 MPa9.4 ksi

Compressive Modulus

2.6 GPa0.38 Msi
2.8 GPa0.41 Msi
2.3 GPa0.33 Msi

Shear Strength

62 MPa9 ksi
60 MPa8.7 ksi
40 MPa5.8 ksi

Fracture Toughness (K_IC)

3.5 MPa·√m3.2 ksi·√in
3 MPa·√m2.7 ksi·√in
3.5 MPa·√m3.2 ksi·√in

Hardness, Rockwell R

119 HRR
120 HRR
115 HRR

Physical

Density and transition temperatures.

Density

1.18 g/cm³0.04 lb/in³
1.14 g/cm³0.04 lb/in³
1.14 g/cm³0.04 lb/in³
1.15 g/cm³0.04 lb/in³

Glass Transition (Tg)

53°C127 °F
58°C136 °F
70°C158 °F
125°C257 °F

Water Absorption (24 h)

1.3%
1.7%
1.3%
0.2%

Melting Temperature (Tm)

220°C428 °F
262°C504 °F

Water Absorption (Saturation)

9%
8.5%
0.6%

Refractive Index

1.53
1.53

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.2 W/m·K0.12 BTU/hr·ft·°F
0.25 W/m·K0.14 BTU/hr·ft·°F
0.25 W/m·K0.14 BTU/hr·ft·°F
0.2 W/m·K0.12 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

80 µm/m·K44.4 µin/in·°F
90 µm/m·K50 µin/in·°F
85 µm/m·K47.2 µin/in·°F
75 µm/m·K41.7 µin/in·°F

Max Service Temperature (continuous)

45°C113 °F
90°C194 °F
100°C212 °F
100°C212 °F

Heat Deflection Temp. @ 0.45 MPa

48°C118 °F
170°C338 °F
220°C428 °F
120°C248 °F

Heat Deflection Temp. @ 1.8 MPa

47°C117 °F
65°C149 °F
80°C176 °F
105°C221 °F

Max Service Temperature (short-term)

55°C131 °F
150°C302 °F
170°C338 °F
125°C257 °F

Specific Heat Capacity

1,700 J/kg·K0.41 BTU/lb·°F
1,670 J/kg·K0.4 BTU/lb·°F
1,400 J/kg·K0.33 BTU/lb·°F

Min Service Temperature

-30°C-22 °F
-40°C-40 °F
-40°C-40 °F

Vicat Softening Point (B50)

190°C374 °F
200°C392 °F
135°C275 °F

Limiting Oxygen Index

24%
25%
23%

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹⁴ Ω·m3.94×10²¹ µΩ·in

Dielectric Strength

25 kV/mm635 V/mil
22 kV/mm559 V/mil
25 kV/mm635 V/mil

Dielectric Constant (1 MHz)

3.7
3.4
3

Dissipation Factor (1 MHz)

0.025
0.02
0.008

Volume Resistivity

1×10¹⁴ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁶ Ω·cm

Surface Resistivity

1×10¹³ Ω
1×10¹³ Ω
1×10¹⁵ Ω

Comparative Tracking Index (CTI)

600 V
600 V
250 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

55 / 100
70 / 100
60 / 100
78 / 100

UV / Weathering Resistance

20 / 100
30 / 100
30 / 100
30 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

55 / 100
68 / 100
65 / 100
65 / 100

Weldability

5 / 100
62 / 100
70 / 100
72 / 100

Formability (cold)

5 / 100
60 / 100
50 / 100
60 / 100

Polishability

70 / 100
55 / 100
60 / 100
65 / 100

Mold Shrinkage

1.2%
1.5%
0.6%

Melt Flow Rate

15 g/10 min
30 g/10 min
14 g/10 min

Processing Melt Temperature (typ.)

260°C500 °F
290°C554 °F
265°C509 °F

Mold Temperature (typ.)

80°C176 °F
80°C176 °F
75°C167 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

115 MJ/kg49,441 BTU/lb
125 MJ/kg53,740 BTU/lb
120 MJ/kg51,591 BTU/lb
100 MJ/kg42,992 BTU/lb

Embodied Carbon (primary production)

6.5 kg CO₂/kg
7.6 kg CO₂/kg
6.7 kg CO₂/kg
4.6 kg CO₂/kg

Typical Recycled Content

0%
5%
5%
15%

Embodied Water

400 L/kg47.9 gal/lb
300 L/kg35.9 gal/lb
200 L/kg24 gal/lb

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

49 kN·m/kg
70 kN·m/kg
72 kN·m/kg
49 kN·m/kg

Specific Stiffness (E / density)

2.1 MN·m/kg
2.6 MN·m/kg
2.6 MN·m/kg
2.1 MN·m/kg

Same in both: Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scalePA6PA66PC-ABSVero

Manufacturing and finishing

CapabilityVeroPA6PA66PC-ABS
3D printingYes
CNC machiningYesYesYes
Sheet metalYesYesYes
Injection moldingYesYesYes
Default conditionVivid ColorsUnfilledUnfilledUnfilled
Relative cost$$$$$ Specialty$ Budget$$ Standard$$ Standard
Min. machined wall0.5 mm0.5 mm0.5 mm
Best machined surfaceRa 0.8 µmRa 0.8 µmRa 0.8 µm
Chrome Plating (Plastic)YesYesYes
Conductive CoatingYes
Dyeing (Nylon)Yes
Primer CoatingYes
Spray PaintingYesYesYes
Tinted CoatingYes
Vacuum MetallizationYes
Waterproof CoatingYes

They share 4 finishes: EMI Shielding Coating, Painting, Soft Touch Coating, UV Coating.

Ready to make it?

Upload a CAD file and FabDigit prices the part in Vero and PA6 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.