FabDigit

THV vs FEP and 2 more: properties

THVFEPPCTFEPFA

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

0.2 GPa0.03 Msi
0.48 GPa0.07 Msi
1.5 GPa0.22 Msi
0.6 GPa0.09 Msi

Poisson's Ratio

0.42
0.45
0.42
0.45

Tensile Strength (Ultimate)

25 MPa3.6 ksi
23 MPa3.3 ksi
37 MPa5.4 ksi
30 MPa4.4 ksi

Elongation at Break

500%
320%
110%
330%

Flexural Modulus

0.19 GPa0.03 Msi
0.6 GPa0.09 Msi
1.5 GPa0.22 Msi
0.62 GPa0.09 Msi

Hardness, Shore D

54 Shore D
56 Shore D
78 Shore D
60 Shore D

Shear Modulus

0.18 GPa0.03 Msi

Yield Strength (0.2% offset)

13 MPa1.9 ksi
34 MPa4.9 ksi
14 MPa2 ksi

Compressive Strength

16 MPa2.3 ksi
40 MPa5.8 ksi
12 MPa1.7 ksi

Izod Impact, Notched

2,700 J/m50.6 ft·lbf/in
145 J/m2.7 ft·lbf/in
1,300 J/m24.3 ft·lbf/in

Hardness, Rockwell R

25 HRR
112 HRR
50 HRR

Compressive Modulus

1.4 GPa0.2 Msi

Flexural Strength

60 MPa8.7 ksi
17 MPa2.5 ksi

Shear Strength

33 MPa4.8 ksi
17 MPa2.5 ksi

Hardness, Shore A

97 Shore A

Physical

Density and transition temperatures.

Density

1.97 g/cm³0.07 lb/in³
2.15 g/cm³0.08 lb/in³
2.12 g/cm³0.08 lb/in³
2.15 g/cm³0.08 lb/in³

Melting Temperature (Tm)

165°C329 °F
260°C500 °F
212°C414 °F
305°C581 °F

Glass Transition (Tg)

0°C32 °F
-90°C-130 °F
50°C122 °F
90°C194 °F

Water Absorption (24 h)

0.03%
0.01%
0.01%
0.02%

Refractive Index

1.355
1.344
1.43
1.35

Light Transmission

92%
95%
92%

Water Absorption (Saturation)

0.01%
0.01%
0.03%

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.2 W/m·K0.12 BTU/hr·ft·°F
0.2 W/m·K0.12 BTU/hr·ft·°F
0.22 W/m·K0.13 BTU/hr·ft·°F
0.22 W/m·K0.13 BTU/hr·ft·°F

Specific Heat Capacity

1,100 J/kg·K0.26 BTU/lb·°F
1,170 J/kg·K0.28 BTU/lb·°F
900 J/kg·K0.21 BTU/lb·°F
1,100 J/kg·K0.26 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

130 µm/m·K72.2 µin/in·°F
100 µm/m·K55.6 µin/in·°F
65 µm/m·K36.1 µin/in·°F
130 µm/m·K72.2 µin/in·°F

Max Service Temperature (continuous)

130°C266 °F
200°C392 °F
135°C275 °F
260°C500 °F

Min Service Temperature

-50°C-58 °F
-200°C-328 °F
-240°C-400 °F
-200°C-328 °F

Heat Deflection Temp. @ 0.45 MPa

50°C122 °F
70°C158 °F
126°C259 °F
74°C165 °F

Limiting Oxygen Index

70%
95%
95%
95%

Max Service Temperature (short-term)

150°C302 °F
230°C446 °F
180°C356 °F
285°C545 °F

Heat Deflection Temp. @ 1.8 MPa

51°C124 °F
78°C172 °F
48°C118 °F

Vicat Softening Point (B50)

150°C302 °F
95°C203 °F

Electrical

Conductivity and insulation.

Dielectric Strength

25 kV/mm635 V/mil
24 kV/mm610 V/mil
21 kV/mm533 V/mil
25 kV/mm635 V/mil

Dielectric Constant (1 MHz)

6
2.1
2.5
2.1

Dissipation Factor (1 MHz)

0.06
6×10⁻⁴
0.014
2×10⁻⁴

Volume Resistivity

1×10¹⁵ Ω·cm
1×10¹⁸ Ω·cm
1×10¹⁸ Ω·cm
1×10¹⁸ Ω·cm

Electrical Resistivity

1×10¹⁶ Ω·m3.94×10²³ µΩ·in
1×10¹⁶ Ω·m3.94×10²³ µΩ·in
1×10¹⁶ Ω·m3.94×10²³ µΩ·in

Surface Resistivity

1×10¹⁶ Ω
1×10¹⁶ Ω
1×10¹⁷ Ω

Same in both: Comparative Tracking Index (CTI) 600 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

92 / 100
98 / 100
95 / 100
100 / 100

UV / Weathering Resistance

95 / 100
98 / 100
92 / 100
99 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

45 / 100
55 / 100
70 / 100
55 / 100

Weldability

85 / 100
80 / 100
20 / 100
78 / 100

Formability (cold)

90 / 100
75 / 100
45 / 100
70 / 100

Polishability

55 / 100
45 / 100
55 / 100
45 / 100

Mold Shrinkage

3%
4%
1.8%
4.2%

Melt Flow Rate

15 g/10 min
7 g/10 min
5 g/10 min

Processing Melt Temperature (typ.)

250°C482 °F
350°C662 °F
290°C554 °F
370°C698 °F

Mold Temperature (typ.)

60°C140 °F
200°C392 °F
120°C248 °F
180°C356 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

230 MJ/kg98,882 BTU/lb
220 MJ/kg94,583 BTU/lb
240 MJ/kg103,182 BTU/lb
250 MJ/kg107,481 BTU/lb

Embodied Carbon (primary production)

13 kg CO₂/kg
12 kg CO₂/kg
13 kg CO₂/kg
12 kg CO₂/kg

Embodied Water

350 L/kg41.9 gal/lb
300 L/kg35.9 gal/lb
400 L/kg47.9 gal/lb
300 L/kg35.9 gal/lb

Same in both: Typical Recycled Content 0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

13 kN·m/kg
11 kN·m/kg
17 kN·m/kg
14 kN·m/kg

Specific Stiffness (E / density)

0.1 MN·m/kg
0.2 MN·m/kg
0.7 MN·m/kg
0.3 MN·m/kg

Same in both: Thermal Diffusivity 0.1 mm²/s · Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scaleFEPPCTFEPFA

Manufacturing and finishing

CapabilityTHVFEPPCTFEPFA
CNC machiningYesYesYes
Sheet metalYesYesYes
Injection moldingYesYesYes
Default conditionUnfilledUnfilledHigh Purity (Semiconductor)
Relative cost$$$$ High$$$$$ Specialty$$$$$ Specialty$$$$$ Specialty
Min. machined wall0.5 mm0.5 mm0.5 mm
Best machined surfaceRa 0.8 µmRa 0.8 µmRa 0.8 µm
Chrome Plating (Plastic)YesYesYes
EMI Shielding CoatingYesYesYes
PaintingYesYesYes
Soft Touch CoatingYesYesYes
Spray PaintingYesYesYes
UV CoatingYesYesYes

Ready to make it?

Upload a CAD file and FabDigit prices the part in THV and FEP side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.