FabDigit

PEKK-ESD vs PPS and 2 more: properties

PEKK-ESDPPSPIPBI

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

3.5 GPa0.51 Msi
3.8 GPa0.55 Msi
3 GPa0.44 Msi
5.9 GPa0.86 Msi

Shear Modulus

1.3 GPa0.18 Msi
1.4 GPa0.2 Msi
1.1 GPa0.16 Msi

Poisson's Ratio

0.4
0.37
0.41
0.34

Tensile Strength (Ultimate)

82 MPa11.9 ksi
78 MPa11.3 ksi
86 MPa12.5 ksi
160 MPa23.2 ksi

Yield Strength (0.2% offset)

78 MPa11.3 ksi
75 MPa10.9 ksi

Elongation at Break

3%
5%
7.5%
3%

Compressive Strength

115 MPa16.7 ksi
120 MPa17.4 ksi
130 MPa18.9 ksi
400 MPa58 ksi

Compressive Modulus

3.2 GPa0.46 Msi
3.5 GPa0.51 Msi
2.9 GPa0.42 Msi
5.8 GPa0.84 Msi

Flexural Strength

128 MPa18.6 ksi
130 MPa18.9 ksi
110 MPa16 ksi
220 MPa31.9 ksi

Flexural Modulus

3.6 GPa0.52 Msi
3.9 GPa0.57 Msi
3.1 GPa0.45 Msi
6.5 GPa0.94 Msi

Shear Strength

55 MPa8 ksi
65 MPa9.4 ksi
80 MPa11.6 ksi
100 MPa14.5 ksi

Fracture Toughness (K_IC)

3.2 MPa·√m2.9 ksi·√in
2 MPa·√m1.8 ksi·√in

Izod Impact, Notched

32 J/m0.6 ft·lbf/in
25 J/m0.47 ft·lbf/in
43 J/m0.81 ft·lbf/in
32 J/m0.6 ft·lbf/in

Hardness, Shore D

86 Shore D
88 Shore D
88 Shore D

Hardness, Rockwell M

100 HRM
95 HRM
105 HRM
125 HRM

Hardness, Rockwell R

125 HRR
123 HRR

Bulk Modulus

6 GPa0.8 Msi

Physical

Density and transition temperatures.

Density

1.33 g/cm³0.05 lb/in³
1.35 g/cm³0.05 lb/in³
1.43 g/cm³0.05 lb/in³
1.3 g/cm³0.05 lb/in³

Melting Temperature (Tm)

305°C581 °F
280°C536 °F

Glass Transition (Tg)

162°C324 °F
88°C190 °F
385°C725 °F
427°C801 °F

Water Absorption (24 h)

0.14%
0.03%
0.3%
0.4%

Water Absorption (Saturation)

0.5%
0.1%
1.2%
5%

Refractive Index

1.7

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.3 W/m·K0.17 BTU/hr·ft·°F
0.29 W/m·K0.17 BTU/hr·ft·°F
0.29 W/m·K0.17 BTU/hr·ft·°F
0.41 W/m·K0.24 BTU/hr·ft·°F

Specific Heat Capacity

1,050 J/kg·K0.25 BTU/lb·°F
1,000 J/kg·K0.24 BTU/lb·°F
1,130 J/kg·K0.27 BTU/lb·°F
1,000 J/kg·K0.24 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

42 µm/m·K23.3 µin/in·°F
52 µm/m·K28.9 µin/in·°F
52 µm/m·K28.9 µin/in·°F
23 µm/m·K12.8 µin/in·°F

Max Service Temperature (continuous)

220°C428 °F
220°C428 °F
260°C500 °F
310°C590 °F

Min Service Temperature

-50°C-58 °F
-40°C-40 °F
-240°C-400 °F
-196°C-321 °F

Heat Deflection Temp. @ 0.45 MPa

175°C347 °F
240°C464 °F
400°C752 °F

Heat Deflection Temp. @ 1.8 MPa

158°C316 °F
110°C230 °F
360°C680 °F
435°C815 °F

Vicat Softening Point (B50)

170°C338 °F

Limiting Oxygen Index

40%
47%
45%
58%

Max Service Temperature (short-term)

280°C536 °F
260°C500 °F
480°C896 °F
500°C932 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

10,000 Ω·m3.94×10¹¹ µΩ·in
1×10¹⁴ Ω·m3.94×10²¹ µΩ·in
1×10¹⁴ Ω·m3.94×10²¹ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in

Volume Resistivity

1,000,000 Ω·cm
1×10¹⁶ Ω·cm
1×10¹⁶ Ω·cm
1×10¹⁴ Ω·cm

Surface Resistivity

1×10⁸ Ω
1×10¹⁵ Ω
1×10¹⁵ Ω

Dielectric Strength

18 kV/mm457 V/mil
22 kV/mm559 V/mil
22 kV/mm559 V/mil

Dielectric Constant (1 MHz)

3.1
3.5
3.2

Dissipation Factor (1 MHz)

0.0013
0.0034
0.004

Comparative Tracking Index (CTI)

175 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

92 / 100
92 / 100
85 / 100
92 / 100

UV / Weathering Resistance

70 / 100
35 / 100
60 / 100
70 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

62 / 100
60 / 100
65 / 100
50 / 100

Weldability

30 / 100
30 / 100
5 / 100
5 / 100

Formability (cold)

20 / 100
15 / 100
15 / 100
5 / 100

Polishability

50 / 100
60 / 100
60 / 100
55 / 100

Mold Shrinkage

1%
1.2%

Melt Flow Rate

4 g/10 min

Processing Melt Temperature (typ.)

390°C734 °F
320°C608 °F

Mold Temperature (typ.)

190°C374 °F
140°C284 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

350 MJ/kg150,473 BTU/lb
115 MJ/kg49,441 BTU/lb
290 MJ/kg124,678 BTU/lb

Embodied Carbon (primary production)

18 kg CO₂/kg
6.2 kg CO₂/kg
13 kg CO₂/kg

Embodied Water

600 L/kg71.9 gal/lb
300 L/kg35.9 gal/lb
600 L/kg71.9 gal/lb

Typical Recycled Content

0%
2%
0%
0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

62 kN·m/kg
58 kN·m/kg
60 kN·m/kg
123 kN·m/kg

Specific Stiffness (E / density)

2.6 MN·m/kg
2.8 MN·m/kg
2.1 MN·m/kg
4.5 MN·m/kg

Thermal Diffusivity

0.2 mm²/s
0.2 mm²/s
0.2 mm²/s
0.3 mm²/s

Same in both: Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scaleStratasys Antero 840CN03PIPBIPPS

Manufacturing and finishing

CapabilityPEKK-ESDPPSPIPBI
3D printingYes
CNC machiningYesYesYes
Sheet metalYesYesYes
Injection moldingYesYesYes
Default conditionUnfilledUnfilledUnfilled
Relative cost$$$$$ Specialty$$$$$ Specialty$$$$$ Specialty$$$$$ Specialty
Min. machined wall0.5 mm0.5 mm0.5 mm
Best machined surfaceRa 0.8 µmRa 0.8 µmRa 0.8 µm
Chrome Plating (Plastic)YesYesYes
Conductive CoatingYes
Dyeing (Nylon)Yes
Primer CoatingYes
Spray PaintingYesYesYes
Tinted CoatingYes
Vacuum MetallizationYes
Waterproof CoatingYes

They share 4 finishes: EMI Shielding Coating, Painting, Soft Touch Coating, UV Coating.

Ready to make it?

Upload a CAD file and FabDigit prices the part in PEKK-ESD and PPS side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.