FabDigit

PEEK vs PPS and 2 more: properties

PEEKPPSPIPEKK

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

3.7 GPa0.54 Msi
3.8 GPa0.55 Msi
3 GPa0.44 Msi
3.9 GPa0.57 Msi

Shear Modulus

1.3 GPa0.19 Msi
1.4 GPa0.2 Msi
1.1 GPa0.16 Msi
1.4 GPa0.2 Msi

Bulk Modulus

6 GPa0.87 Msi
6 GPa0.8 Msi
7 GPa0.94 Msi

Poisson's Ratio

0.4
0.37
0.41
0.4

Tensile Strength (Ultimate)

100 MPa14.5 ksi
78 MPa11.3 ksi
86 MPa12.5 ksi
95 MPa13.8 ksi

Yield Strength (0.2% offset)

100 MPa14.5 ksi
75 MPa10.9 ksi
95 MPa13.8 ksi

Elongation at Break

30%
5%
7.5%
8%

Compressive Strength

130 MPa18.9 ksi
120 MPa17.4 ksi
130 MPa18.9 ksi
130 MPa18.9 ksi

Compressive Modulus

3.6 GPa0.52 Msi
3.5 GPa0.51 Msi
2.9 GPa0.42 Msi
3.5 GPa0.51 Msi

Flexural Strength

165 MPa23.9 ksi
130 MPa18.9 ksi
110 MPa16 ksi
150 MPa21.8 ksi

Flexural Modulus

4 GPa0.58 Msi
3.9 GPa0.57 Msi
3.1 GPa0.45 Msi
3.9 GPa0.57 Msi

Shear Strength

55 MPa8 ksi
65 MPa9.4 ksi
80 MPa11.6 ksi
65 MPa9.4 ksi

Fracture Toughness (K_IC)

3.5 MPa·√m3.2 ksi·√in
2 MPa·√m1.8 ksi·√in
3.5 MPa·√m3.2 ksi·√in

Izod Impact, Notched

75 J/m1.4 ft·lbf/in
25 J/m0.47 ft·lbf/in
43 J/m0.81 ft·lbf/in
50 J/m0.94 ft·lbf/in

Hardness, Shore D

86 Shore D
88 Shore D
88 Shore D
86 Shore D

Hardness, Rockwell M

99 HRM
95 HRM
105 HRM
100 HRM

Hardness, Rockwell R

126 HRR
123 HRR

Physical

Density and transition temperatures.

Density

1.3 g/cm³0.05 lb/in³
1.35 g/cm³0.05 lb/in³
1.43 g/cm³0.05 lb/in³
1.3 g/cm³0.05 lb/in³

Melting Temperature (Tm)

343°C649 °F
280°C536 °F
332°C630 °F

Glass Transition (Tg)

143°C289 °F
88°C190 °F
385°C725 °F
162°C324 °F

Water Absorption (24 h)

0.12%
0.03%
0.3%
0.15%

Water Absorption (Saturation)

0.45%
0.1%
1.2%
0.5%

Refractive Index

1.7

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.25 W/m·K0.14 BTU/hr·ft·°F
0.29 W/m·K0.17 BTU/hr·ft·°F
0.29 W/m·K0.17 BTU/hr·ft·°F
0.26 W/m·K0.15 BTU/hr·ft·°F

Specific Heat Capacity

1,340 J/kg·K0.32 BTU/lb·°F
1,000 J/kg·K0.24 BTU/lb·°F
1,130 J/kg·K0.27 BTU/lb·°F
1,050 J/kg·K0.25 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

47 µm/m·K26.1 µin/in·°F
52 µm/m·K28.9 µin/in·°F
52 µm/m·K28.9 µin/in·°F
48 µm/m·K26.7 µin/in·°F

Max Service Temperature (continuous)

250°C482 °F
220°C428 °F
260°C500 °F
240°C464 °F

Min Service Temperature

-60°C-76 °F
-40°C-40 °F
-240°C-400 °F
-60°C-76 °F

Heat Deflection Temp. @ 0.45 MPa

315°C599 °F
240°C464 °F
400°C752 °F
175°C347 °F

Heat Deflection Temp. @ 1.8 MPa

152°C306 °F
110°C230 °F
360°C680 °F
160°C320 °F

Vicat Softening Point (B50)

315°C599 °F

Limiting Oxygen Index

35%
47%
45%
40%

Max Service Temperature (short-term)

300°C572 °F
260°C500 °F
480°C896 °F
300°C572 °F

Electrical

Conductivity and insulation.

Dielectric Strength

21 kV/mm533 V/mil
18 kV/mm457 V/mil
22 kV/mm559 V/mil
22 kV/mm559 V/mil

Dielectric Constant (1 MHz)

3.2
3.1
3.5
3.3

Dissipation Factor (1 MHz)

0.003
0.0013
0.0034
0.004

Comparative Tracking Index (CTI)

150 V
175 V
175 V

Same in both: Electrical Resistivity 1×10¹⁴ Ω·m3.94×10²¹ µΩ·in · Volume Resistivity 1×10¹⁶ Ω·cm · Surface Resistivity 1×10¹⁵ Ω

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

90 / 100
92 / 100
85 / 100
92 / 100

UV / Weathering Resistance

45 / 100
35 / 100
60 / 100
45 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

70 / 100
60 / 100
65 / 100
60 / 100

Weldability

45 / 100
30 / 100
5 / 100
55 / 100

Formability (cold)

30 / 100
15 / 100
15 / 100
35 / 100

Polishability

70 / 100
60 / 100
60 / 100
60 / 100

Mold Shrinkage

1.2%
1.2%
1.2%

Melt Flow Rate

3 g/10 min

Processing Melt Temperature (typ.)

380°C716 °F
320°C608 °F
380°C716 °F

Mold Temperature (typ.)

180°C356 °F
140°C284 °F
200°C392 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

290 MJ/kg124,678 BTU/lb
115 MJ/kg49,441 BTU/lb
290 MJ/kg124,678 BTU/lb
330 MJ/kg141,875 BTU/lb

Embodied Carbon (primary production)

15 kg CO₂/kg
6.2 kg CO₂/kg
13 kg CO₂/kg
18 kg CO₂/kg

Embodied Water

450 L/kg53.9 gal/lb
300 L/kg35.9 gal/lb
600 L/kg71.9 gal/lb
500 L/kg59.9 gal/lb

Typical Recycled Content

0%
2%
0%
0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

77 kN·m/kg
58 kN·m/kg
60 kN·m/kg
73 kN·m/kg

Specific Stiffness (E / density)

2.8 MN·m/kg
2.8 MN·m/kg
2.1 MN·m/kg
3 MN·m/kg

Thermal Diffusivity

0.1 mm²/s
0.2 mm²/s
0.2 mm²/s
0.2 mm²/s

Same in both: Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scalePIPEEKPEKKPPS

Manufacturing and finishing

CapabilityPEEKPPSPIPEKK
CNC machiningYesYesYes
Sheet metalYesYesYes
Injection moldingYesYesYes
3D printingYesYes
Default conditionVirginUnfilledUnfilledUnfilled
Relative cost$$$$$ Specialty$$$$$ Specialty$$$$$ Specialty$$$$$ Specialty
Min. machined wall0.8 mm0.5 mm0.5 mm
Best machined surfaceRa 0.8 µmRa 0.8 µmRa 0.8 µm
Chrome Plating (Plastic)YesYesYes
Conductive CoatingYesYes
Dyeing (Nylon)YesYes
Primer CoatingYesYes
Spray PaintingYesYesYes
Tinted CoatingYesYes
Vacuum MetallizationYesYes
Waterproof CoatingYesYes

They share 4 finishes: EMI Shielding Coating, Painting, Soft Touch Coating, UV Coating.

Ready to make it?

Upload a CAD file and FabDigit prices the part in PEEK and PPS side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.