FabDigit

IR vs NR and 2 more: properties

IRNREPDMSilicone

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

0 GPa2.61×10⁻⁴ Msi
0 GPa2.18×10⁻⁴ Msi
0.01 GPa8.7×10⁻⁴ Msi
0 GPa3.19×10⁻⁴ Msi

Shear Modulus

7×10⁻⁴ GPa1.02×10⁻⁴ Msi
7×10⁻⁴ GPa1.02×10⁻⁴ Msi
0 GPa2.9×10⁻⁴ Msi
7.5×10⁻⁴ GPa1.09×10⁻⁴ Msi

Bulk Modulus

2 GPa0.29 Msi
2 GPa0.29 Msi
2 GPa0.29 Msi
2 GPa0.22 Msi

Poisson's Ratio

0.5
0.5
0.5
0.49

Tensile Strength (Ultimate)

22 MPa3.2 ksi
24 MPa3.5 ksi
12 MPa1.7 ksi
8 MPa1.2 ksi

Elongation at Break

750%
750%
400%
500%

Hardness, Shore A

50 Shore A
40 Shore A
70 Shore A
50 Shore A

Tear Strength

40 kN/m228 lbf/in
35 kN/m200 lbf/in
25 kN/m143 lbf/in
25 kN/m143 lbf/in

Compression Set (22 h, 70 °C)

25%
25%
20%
20%

Shear Strength

6 MPa0.87 ksi

Hardness, Shore D

22 Shore D

Physical

Density and transition temperatures.

Density

0.93 g/cm³0.03 lb/in³
0.97 g/cm³0.04 lb/in³
1.15 g/cm³0.04 lb/in³
1.15 g/cm³0.04 lb/in³

Glass Transition (Tg)

-70°C-94 °F
-70°C-94 °F
-55°C-67 °F
-125°C-193 °F

Water Absorption (24 h)

1%
1%
0.5%
0.3%

Refractive Index

1.52
1.52
1.41

Water Absorption (Saturation)

3.5%

Light Transmission

88%

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.14 W/m·K0.08 BTU/hr·ft·°F
0.14 W/m·K0.08 BTU/hr·ft·°F
0.3 W/m·K0.17 BTU/hr·ft·°F
0.22 W/m·K0.13 BTU/hr·ft·°F

Specific Heat Capacity

1,900 J/kg·K0.45 BTU/lb·°F
1,900 J/kg·K0.45 BTU/lb·°F
2,000 J/kg·K0.48 BTU/lb·°F
1,300 J/kg·K0.31 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

220 µm/m·K122 µin/in·°F
220 µm/m·K122 µin/in·°F
180 µm/m·K100 µin/in·°F
270 µm/m·K150 µin/in·°F

Max Service Temperature (continuous)

80°C176 °F
80°C176 °F
120°C248 °F
200°C392 °F

Min Service Temperature

-55°C-67 °F
-50°C-58 °F
-50°C-58 °F
-60°C-76 °F

Limiting Oxygen Index

18%
18%
19%
26%

Max Service Temperature (short-term)

110°C230 °F
100°C212 °F
160°C320 °F
250°C482 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹³ Ω·m3.94×10²⁰ µΩ·in
1×10¹⁴ Ω·m3.94×10²¹ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹³ Ω·m3.94×10²⁰ µΩ·in

Dielectric Strength

22 kV/mm559 V/mil
22 kV/mm559 V/mil
25 kV/mm635 V/mil
22 kV/mm559 V/mil

Dielectric Constant (1 MHz)

2.6
2.7
3
3

Dissipation Factor (1 MHz)

0.003
0.003
0.007
0.002

Volume Resistivity

1×10¹⁵ Ω·cm
1×10¹⁵ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁵ Ω·cm

Surface Resistivity

1×10¹⁴ Ω
1×10¹⁴ Ω

Comparative Tracking Index (CTI)

600 V
600 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

50 / 100
70 / 100
85 / 100
90 / 100

UV / Weathering Resistance

20 / 100
20 / 100
95 / 100
97 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

25 / 100
20 / 100
30 / 100
20 / 100

Formability (cold)

95 / 100
95 / 100
90 / 100
95 / 100

Mold Shrinkage

2.3%
2.2%
2.5%
2.5%

Mold Temperature (typ.)

165°C329 °F
150°C302 °F
175°C347 °F
180°C356 °F

Weldability

15 / 100
15 / 100
20 / 100

Polishability

30 / 100
20 / 100
85 / 100

Processing Melt Temperature (typ.)

100°C212 °F
25°C77 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

95 MJ/kg40,843 BTU/lb
65 MJ/kg27,945 BTU/lb
95 MJ/kg40,843 BTU/lb
110 MJ/kg47,292 BTU/lb

Embodied Carbon (primary production)

3.5 kg CO₂/kg
1.9 kg CO₂/kg
4 kg CO₂/kg
6.5 kg CO₂/kg

Embodied Water

200 L/kg24 gal/lb
1,000 L/kg120 gal/lb
150 L/kg18 gal/lb
250 L/kg30 gal/lb

Typical Recycled Content

0%
5%
5%
0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

24 kN·m/kg
25 kN·m/kg
10 kN·m/kg
7 kN·m/kg

Thermal Shock Resistance Index

8
10
3
3

Same in both: Specific Stiffness (E / density) 0 MN·m/kg · Thermal Diffusivity 0.1 mm²/s

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scaleEPDMSilicone

Manufacturing and finishing

CapabilityIRNREPDMSilicone
Injection moldingYesYes
Default conditionSolidMedical Grade
Relative cost$$ Standard$$ Standard$$ Standard$$$ Premium
Min. machined wall
Best machined surface
Chrome Plating (Plastic)YesYes
EMI Shielding CoatingYesYes
Soft Touch CoatingYesYes
Spray PaintingYesYes
UV CoatingYesYes

Ready to make it?

Upload a CAD file and FabDigit prices the part in IR and NR side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.