FabDigit

DAIP vs DAP and 2 more: properties

DAIPDAPPBIEpoxy

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

11 GPa1.6 Msi
10.5 GPa1.5 Msi
5.9 GPa0.86 Msi
3 GPa0.44 Msi

Poisson's Ratio

0.34
0.32
0.34
0.35

Tensile Strength (Ultimate)

55 MPa8 ksi
55 MPa8 ksi
160 MPa23.2 ksi
65 MPa9.4 ksi

Elongation at Break

0.6%
0.6%
3%
4%

Compressive Strength

200 MPa29 ksi
200 MPa29 ksi
400 MPa58 ksi
110 MPa16 ksi

Flexural Strength

105 MPa15.2 ksi
105 MPa15.2 ksi
220 MPa31.9 ksi
110 MPa16 ksi

Flexural Modulus

11.5 GPa1.7 Msi
11 GPa1.6 Msi
6.5 GPa0.94 Msi
3 GPa0.44 Msi

Izod Impact, Notched

75 J/m1.4 ft·lbf/in
40 J/m0.75 ft·lbf/in
32 J/m0.6 ft·lbf/in
20 J/m0.37 ft·lbf/in

Hardness, Rockwell M

108 HRM
110 HRM
125 HRM
100 HRM

Compressive Modulus

5.8 GPa0.84 Msi
3 GPa0.44 Msi

Shear Strength

100 MPa14.5 ksi
45 MPa6.5 ksi

Shear Modulus

1.2 GPa0.17 Msi

Bulk Modulus

5 GPa0.65 Msi

Fracture Toughness (K_IC)

0.6 MPa·√m0.55 ksi·√in

Hardness, Shore D

85 Shore D

Physical

Density and transition temperatures.

Density

1.8 g/cm³0.07 lb/in³
1.8 g/cm³0.07 lb/in³
1.3 g/cm³0.05 lb/in³
1.2 g/cm³0.04 lb/in³

Glass Transition (Tg)

190°C374 °F
160°C320 °F
427°C801 °F
120°C248 °F

Water Absorption (24 h)

0.25%
0.2%
0.4%
0.15%

Water Absorption (Saturation)

0.7%
0.6%
5%
1.6%

Refractive Index

1.56

Light Transmission

88%

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.42 W/m·K0.24 BTU/hr·ft·°F
0.5 W/m·K0.29 BTU/hr·ft·°F
0.41 W/m·K0.24 BTU/hr·ft·°F
0.2 W/m·K0.12 BTU/hr·ft·°F

Specific Heat Capacity

1,150 J/kg·K0.27 BTU/lb·°F
1,050 J/kg·K0.25 BTU/lb·°F
1,000 J/kg·K0.24 BTU/lb·°F
1,100 J/kg·K0.26 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

30 µm/m·K16.7 µin/in·°F
25 µm/m·K13.9 µin/in·°F
23 µm/m·K12.8 µin/in·°F
60 µm/m·K33.3 µin/in·°F

Max Service Temperature (continuous)

205°C401 °F
180°C356 °F
310°C590 °F
130°C266 °F

Min Service Temperature

-65°C-85 °F
-60°C-76 °F
-196°C-321 °F
-50°C-58 °F

Heat Deflection Temp. @ 0.45 MPa

300°C572 °F
285°C545 °F
130°C266 °F

Heat Deflection Temp. @ 1.8 MPa

290°C554 °F
265°C509 °F
435°C815 °F
110°C230 °F

Limiting Oxygen Index

34%
32%
58%
20%

Max Service Temperature (short-term)

260°C500 °F
230°C446 °F
500°C932 °F
180°C356 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹³ Ω·m3.94×10²⁰ µΩ·in
1×10¹³ Ω·m3.94×10²⁰ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹³ Ω·m3.94×10²⁰ µΩ·in

Dielectric Strength

16 kV/mm406 V/mil
16 kV/mm406 V/mil
22 kV/mm559 V/mil
20 kV/mm508 V/mil

Dielectric Constant (1 MHz)

4.4
4.3
3.2
3.6

Dissipation Factor (1 MHz)

0.01
0.011
0.004
0.02

Volume Resistivity

1×10¹⁵ Ω·cm
1×10¹⁵ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁵ Ω·cm

Surface Resistivity

1×10¹⁴ Ω
1×10¹⁴ Ω
1×10¹⁴ Ω

Comparative Tracking Index (CTI)

400 V
200 V
300 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

85 / 100
80 / 100
92 / 100
82 / 100

UV / Weathering Resistance

70 / 100
55 / 100
70 / 100
25 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

40 / 100
40 / 100
50 / 100
55 / 100

Weldability

3 / 100
0 / 100
5 / 100
0 / 100

Formability (cold)

3 / 100
0 / 100
5 / 100
5 / 100

Polishability

45 / 100
45 / 100
55 / 100
75 / 100

Mold Shrinkage

0.35%
0.4%
0.2%

Processing Melt Temperature (typ.)

105°C221 °F

Mold Temperature (typ.)

165°C329 °F
160°C320 °F
165°C329 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

105 MJ/kg45,142 BTU/lb
105 MJ/kg45,142 BTU/lb
137 MJ/kg58,899 BTU/lb

Embodied Carbon (primary production)

5.5 kg CO₂/kg
5.5 kg CO₂/kg
6.6 kg CO₂/kg

Embodied Water

180 L/kg21.6 gal/lb
190 L/kg22.8 gal/lb

Same in both: Typical Recycled Content 0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

31 kN·m/kg
31 kN·m/kg
123 kN·m/kg
54 kN·m/kg

Specific Stiffness (E / density)

6.1 MN·m/kg
5.8 MN·m/kg
4.5 MN·m/kg
2.5 MN·m/kg

Thermal Diffusivity

0.2 mm²/s
0.3 mm²/s
0.3 mm²/s
0.2 mm²/s

Same in both: Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scalePBI

Manufacturing and finishing

CapabilityDAIPDAPPBIEpoxy
CNC machiningYes
Sheet metalYes
Injection moldingYes
Default conditionUnfilled
Relative cost$$$$ High$$$$ High$$$$$ Specialty$$ Standard
Min. machined wall0.5 mm
Best machined surfaceRa 0.8 µm
Chrome Plating (Plastic)Yes
EMI Shielding CoatingYes
PaintingYes
Soft Touch CoatingYes
Spray PaintingYes
UV CoatingYes

Ready to make it?

Upload a CAD file and FabDigit prices the part in DAIP and DAP side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.