FabDigit

CTA vs CN and 2 more: properties

CTACNCACAB

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

3.2 GPa0.46 Msi
1.8 GPa0.26 Msi
1.6 GPa0.23 Msi
1.4 GPa0.2 Msi

Shear Modulus

1.2 GPa0.17 Msi
0.6 GPa0.09 Msi
0.5 GPa0.07 Msi

Poisson's Ratio

0.38
0.4
0.4
0.38

Tensile Strength (Ultimate)

70 MPa10.2 ksi
52 MPa7.5 ksi
40 MPa5.8 ksi
32 MPa4.6 ksi

Yield Strength (0.2% offset)

55 MPa8 ksi
42 MPa6.1 ksi
35 MPa5.1 ksi
28 MPa4.1 ksi

Elongation at Break

25%
35%
30%
60%

Compressive Strength

105 MPa15.2 ksi
62 MPa9 ksi
80 MPa11.6 ksi
45 MPa6.5 ksi

Flexural Strength

85 MPa12.3 ksi
68 MPa9.9 ksi
65 MPa9.4 ksi
45 MPa6.5 ksi

Flexural Modulus

2.9 GPa0.42 Msi
1.7 GPa0.25 Msi
1.8 GPa0.26 Msi
1.3 GPa0.19 Msi

Shear Strength

50 MPa7.3 ksi
40 MPa5.8 ksi
38 MPa5.5 ksi
30 MPa4.4 ksi

Izod Impact, Notched

60 J/m1.1 ft·lbf/in
320 J/m6 ft·lbf/in
110 J/m2.1 ft·lbf/in
200 J/m3.7 ft·lbf/in

Hardness, Rockwell M

65 HRM

Hardness, Rockwell R

115 HRR
105 HRR
100 HRR
95 HRR

Hardness, Shore D

80 Shore D
78 Shore D
75 Shore D

Bulk Modulus

3 GPa0.39 Msi
2 GPa0.32 Msi

Compressive Modulus

1.7 GPa0.25 Msi
1.3 GPa0.19 Msi

Fracture Toughness (K_IC)

2 MPa·√m1.8 ksi·√in
2 MPa·√m1.8 ksi·√in

Physical

Density and transition temperatures.

Density

1.3 g/cm³0.05 lb/in³
1.38 g/cm³0.05 lb/in³
1.3 g/cm³0.05 lb/in³
1.19 g/cm³0.04 lb/in³

Melting Temperature (Tm)

300°C572 °F

Glass Transition (Tg)

185°C365 °F
55°C131 °F
120°C248 °F
115°C239 °F

Water Absorption (24 h)

2.5%
1.8%
2.5%
1.3%

Water Absorption (Saturation)

6%
4.5%
7%
2.6%

Refractive Index

1.475
1.5
1.48
1.475

Light Transmission

92%
88%
90%
89%

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.21 W/m·K0.12 BTU/hr·ft·°F
0.22 W/m·K0.13 BTU/hr·ft·°F
0.22 W/m·K0.13 BTU/hr·ft·°F
0.2 W/m·K0.12 BTU/hr·ft·°F

Specific Heat Capacity

1,500 J/kg·K0.36 BTU/lb·°F
1,500 J/kg·K0.36 BTU/lb·°F
1,600 J/kg·K0.38 BTU/lb·°F
1,600 J/kg·K0.38 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

80 µm/m·K44.4 µin/in·°F
110 µm/m·K61.1 µin/in·°F
130 µm/m·K72.2 µin/in·°F
130 µm/m·K72.2 µin/in·°F

Max Service Temperature (continuous)

95°C203 °F
55°C131 °F
65°C149 °F
70°C158 °F

Min Service Temperature

-40°C-40 °F
-30°C-22 °F
-40°C-40 °F
-40°C-40 °F

Heat Deflection Temp. @ 0.45 MPa

120°C248 °F
68°C154 °F
70°C158 °F
75°C167 °F

Heat Deflection Temp. @ 1.8 MPa

95°C203 °F
52°C126 °F
55°C131 °F
58°C136 °F

Vicat Softening Point (B50)

140°C284 °F
75°C167 °F
75°C167 °F
100°C212 °F

Limiting Oxygen Index

19%
19%
20%

Max Service Temperature (short-term)

140°C284 °F
85°C185 °F
90°C194 °F
95°C203 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹¹ Ω·m3.94×10¹⁸ µΩ·in
1×10¹⁰ Ω·m3.94×10¹⁷ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in

Dielectric Strength

16 kV/mm406 V/mil
16 kV/mm406 V/mil
18 kV/mm457 V/mil
16 kV/mm406 V/mil

Dielectric Constant (1 MHz)

3.4
6
4
3.4

Dissipation Factor (1 MHz)

0.025
0.09
0.04
0.03

Volume Resistivity

1×10¹⁴ Ω·cm
1×10¹³ Ω·cm
1×10¹² Ω·cm
1×10¹⁴ Ω·cm

Surface Resistivity

1×10¹³ Ω
1×10¹³ Ω
1×10¹⁴ Ω

Comparative Tracking Index (CTI)

600 V
600 V
600 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

UV / Weathering Resistance

45 / 100
12 / 100
50 / 100
70 / 100

Corrosion Resistance

45 / 100
55 / 100
50 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

65 / 100
85 / 100
75 / 100
75 / 100

Weldability

60 / 100
70 / 100
55 / 100
60 / 100

Formability (cold)

70 / 100
80 / 100
78 / 100
80 / 100

Polishability

80 / 100
92 / 100
85 / 100
85 / 100

Mold Shrinkage

0.5%
0.5%
0.5%

Processing Melt Temperature (typ.)

245°C473 °F
200°C392 °F
200°C392 °F

Mold Temperature (typ.)

70°C158 °F
55°C131 °F
55°C131 °F

Melt Flow Rate

10 g/10 min

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

105 MJ/kg45,142 BTU/lb
95 MJ/kg40,843 BTU/lb
100 MJ/kg42,992 BTU/lb
105 MJ/kg45,142 BTU/lb

Embodied Carbon (primary production)

4.5 kg CO₂/kg
4.5 kg CO₂/kg
4 kg CO₂/kg
4.5 kg CO₂/kg

Embodied Water

600 L/kg71.9 gal/lb
250 L/kg30 gal/lb
350 L/kg41.9 gal/lb
500 L/kg59.9 gal/lb

Typical Recycled Content

2%
0%
2%
0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

54 kN·m/kg
38 kN·m/kg
31 kN·m/kg
27 kN·m/kg

Specific Stiffness (E / density)

2.5 MN·m/kg
1.3 MN·m/kg
1.2 MN·m/kg
1.2 MN·m/kg

Modulus of Resilience

473 kJ/m³
490 kJ/m³
383 kJ/m³
280 kJ/m³

Same in both: Thermal Diffusivity 0.1 mm²/s · Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scaleCNCTACACAB

Manufacturing and finishing

CapabilityCTACNCACAB
Default condition
Relative cost$$$ Premium$$$ Premium$$$ Premium$$$ Premium
Min. machined wall
Best machined surface

Ready to make it?

Upload a CAD file and FabDigit prices the part in CTA and CN side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.