Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

1.4 GPa0.2 Msi
1.8 GPa0.26 Msi
3.2 GPa0.46 Msi
1.6 GPa0.23 Msi

Shear Modulus

0.5 GPa0.07 Msi
1.2 GPa0.17 Msi
0.6 GPa0.09 Msi

Bulk Modulus

2 GPa0.32 Msi
3 GPa0.39 Msi

Poisson's Ratio

0.38
0.4
0.38
0.4

Tensile Strength (Ultimate)

32 MPa4.6 ksi
52 MPa7.5 ksi
70 MPa10.2 ksi
40 MPa5.8 ksi

Yield Strength (0.2% offset)

28 MPa4.1 ksi
42 MPa6.1 ksi
55 MPa8 ksi
35 MPa5.1 ksi

Elongation at Break

60%
35%
25%
30%

Compressive Strength

45 MPa6.5 ksi
62 MPa9 ksi
105 MPa15.2 ksi
80 MPa11.6 ksi

Compressive Modulus

1.3 GPa0.19 Msi
1.7 GPa0.25 Msi

Flexural Strength

45 MPa6.5 ksi
68 MPa9.9 ksi
85 MPa12.3 ksi
65 MPa9.4 ksi

Flexural Modulus

1.3 GPa0.19 Msi
1.7 GPa0.25 Msi
2.9 GPa0.42 Msi
1.8 GPa0.26 Msi

Shear Strength

30 MPa4.4 ksi
40 MPa5.8 ksi
50 MPa7.3 ksi
38 MPa5.5 ksi

Fracture Toughness (K_IC)

2 MPa·√m1.8 ksi·√in
2 MPa·√m1.8 ksi·√in

Izod Impact, Notched

200 J/m3.7 ft·lbf/in
320 J/m6 ft·lbf/in
60 J/m1.1 ft·lbf/in
110 J/m2.1 ft·lbf/in

Hardness, Shore D

75 Shore D
80 Shore D
78 Shore D

Hardness, Rockwell R

95 HRR
105 HRR
115 HRR
100 HRR

Hardness, Rockwell M

65 HRM

Physical

Density and transition temperatures.

Density

1.19 g/cm³0.04 lb/in³
1.38 g/cm³0.05 lb/in³
1.3 g/cm³0.05 lb/in³
1.3 g/cm³0.05 lb/in³

Glass Transition (Tg)

115°C239 °F
55°C131 °F
185°C365 °F
120°C248 °F

Water Absorption (24 h)

1.3%
1.8%
2.5%
2.5%

Water Absorption (Saturation)

2.6%
4.5%
6%
7%

Refractive Index

1.475
1.5
1.475
1.48

Light Transmission

89%
88%
92%
90%

Melting Temperature (Tm)

300°C572 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.2 W/m·K0.12 BTU/hr·ft·°F
0.22 W/m·K0.13 BTU/hr·ft·°F
0.21 W/m·K0.12 BTU/hr·ft·°F
0.22 W/m·K0.13 BTU/hr·ft·°F

Specific Heat Capacity

1,600 J/kg·K0.38 BTU/lb·°F
1,500 J/kg·K0.36 BTU/lb·°F
1,500 J/kg·K0.36 BTU/lb·°F
1,600 J/kg·K0.38 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

130 µm/m·K72.2 µin/in·°F
110 µm/m·K61.1 µin/in·°F
80 µm/m·K44.4 µin/in·°F
130 µm/m·K72.2 µin/in·°F

Max Service Temperature (continuous)

70°C158 °F
55°C131 °F
95°C203 °F
65°C149 °F

Min Service Temperature

-40°C-40 °F
-30°C-22 °F
-40°C-40 °F
-40°C-40 °F

Heat Deflection Temp. @ 0.45 MPa

75°C167 °F
68°C154 °F
120°C248 °F
70°C158 °F

Heat Deflection Temp. @ 1.8 MPa

58°C136 °F
52°C126 °F
95°C203 °F
55°C131 °F

Vicat Softening Point (B50)

100°C212 °F
75°C167 °F
140°C284 °F
75°C167 °F

Limiting Oxygen Index

20%
19%
19%

Max Service Temperature (short-term)

95°C203 °F
85°C185 °F
140°C284 °F
90°C194 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹¹ Ω·m3.94×10¹⁸ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹⁰ Ω·m3.94×10¹⁷ µΩ·in

Dielectric Strength

16 kV/mm406 V/mil
16 kV/mm406 V/mil
16 kV/mm406 V/mil
18 kV/mm457 V/mil

Dielectric Constant (1 MHz)

3.4
6
3.4
4

Dissipation Factor (1 MHz)

0.03
0.09
0.025
0.04

Volume Resistivity

1×10¹⁴ Ω·cm
1×10¹³ Ω·cm
1×10¹⁴ Ω·cm
1×10¹² Ω·cm

Surface Resistivity

1×10¹⁴ Ω
1×10¹³ Ω
1×10¹³ Ω

Comparative Tracking Index (CTI)

600 V
600 V
600 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

50 / 100
45 / 100
55 / 100

UV / Weathering Resistance

70 / 100
12 / 100
45 / 100
50 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

75 / 100
85 / 100
65 / 100
75 / 100

Weldability

60 / 100
70 / 100
60 / 100
55 / 100

Formability (cold)

80 / 100
80 / 100
70 / 100
78 / 100

Polishability

85 / 100
92 / 100
80 / 100
85 / 100

Mold Shrinkage

0.5%
0.5%
0.5%

Melt Flow Rate

10 g/10 min

Processing Melt Temperature (typ.)

200°C392 °F
245°C473 °F
200°C392 °F

Mold Temperature (typ.)

55°C131 °F
70°C158 °F
55°C131 °F

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

105 MJ/kg45,142 BTU/lb
95 MJ/kg40,843 BTU/lb
105 MJ/kg45,142 BTU/lb
100 MJ/kg42,992 BTU/lb

Embodied Carbon (primary production)

4.5 kg CO₂/kg
4.5 kg CO₂/kg
4.5 kg CO₂/kg
4 kg CO₂/kg

Embodied Water

500 L/kg59.9 gal/lb
250 L/kg30 gal/lb
600 L/kg71.9 gal/lb
350 L/kg41.9 gal/lb

Typical Recycled Content

0%
0%
2%
2%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

27 kN·m/kg
38 kN·m/kg
54 kN·m/kg
31 kN·m/kg

Specific Stiffness (E / density)

1.2 MN·m/kg
1.3 MN·m/kg
2.5 MN·m/kg
1.2 MN·m/kg

Modulus of Resilience

280 kJ/m³
490 kJ/m³
473 kJ/m³
383 kJ/m³

Same in both: Thermal Diffusivity 0.1 mm²/s · Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scaleCNCTACACAB

Manufacturing and finishing

CapabilityCABCNCTACA
Default condition
Relative cost$$$ Premium$$$ Premium$$$ Premium$$$ Premium
Min. machined wall
Best machined surface

Ready to make it?

Upload a CAD file and FabDigit prices the part in CAB and CN side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.