FabDigit

CA vs CN and 2 more: properties

CACNCTACAB

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

1.6 GPa0.23 Msi
1.8 GPa0.26 Msi
3.2 GPa0.46 Msi
1.4 GPa0.2 Msi

Shear Modulus

0.6 GPa0.09 Msi
1.2 GPa0.17 Msi
0.5 GPa0.07 Msi

Bulk Modulus

3 GPa0.39 Msi
2 GPa0.32 Msi

Poisson's Ratio

0.4
0.4
0.38
0.38

Tensile Strength (Ultimate)

40 MPa5.8 ksi
52 MPa7.5 ksi
70 MPa10.2 ksi
32 MPa4.6 ksi

Yield Strength (0.2% offset)

35 MPa5.1 ksi
42 MPa6.1 ksi
55 MPa8 ksi
28 MPa4.1 ksi

Elongation at Break

30%
35%
25%
60%

Compressive Strength

80 MPa11.6 ksi
62 MPa9 ksi
105 MPa15.2 ksi
45 MPa6.5 ksi

Compressive Modulus

1.7 GPa0.25 Msi
1.3 GPa0.19 Msi

Flexural Strength

65 MPa9.4 ksi
68 MPa9.9 ksi
85 MPa12.3 ksi
45 MPa6.5 ksi

Flexural Modulus

1.8 GPa0.26 Msi
1.7 GPa0.25 Msi
2.9 GPa0.42 Msi
1.3 GPa0.19 Msi

Shear Strength

38 MPa5.5 ksi
40 MPa5.8 ksi
50 MPa7.3 ksi
30 MPa4.4 ksi

Fracture Toughness (K_IC)

2 MPa·√m1.8 ksi·√in
2 MPa·√m1.8 ksi·√in

Izod Impact, Notched

110 J/m2.1 ft·lbf/in
320 J/m6 ft·lbf/in
60 J/m1.1 ft·lbf/in
200 J/m3.7 ft·lbf/in

Hardness, Shore D

78 Shore D
80 Shore D
75 Shore D

Hardness, Rockwell R

100 HRR
105 HRR
115 HRR
95 HRR

Hardness, Rockwell M

65 HRM

Physical

Density and transition temperatures.

Density

1.3 g/cm³0.05 lb/in³
1.38 g/cm³0.05 lb/in³
1.3 g/cm³0.05 lb/in³
1.19 g/cm³0.04 lb/in³

Glass Transition (Tg)

120°C248 °F
55°C131 °F
185°C365 °F
115°C239 °F

Water Absorption (24 h)

2.5%
1.8%
2.5%
1.3%

Water Absorption (Saturation)

7%
4.5%
6%
2.6%

Refractive Index

1.48
1.5
1.475
1.475

Light Transmission

90%
88%
92%
89%

Melting Temperature (Tm)

300°C572 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

0.22 W/m·K0.13 BTU/hr·ft·°F
0.22 W/m·K0.13 BTU/hr·ft·°F
0.21 W/m·K0.12 BTU/hr·ft·°F
0.2 W/m·K0.12 BTU/hr·ft·°F

Specific Heat Capacity

1,600 J/kg·K0.38 BTU/lb·°F
1,500 J/kg·K0.36 BTU/lb·°F
1,500 J/kg·K0.36 BTU/lb·°F
1,600 J/kg·K0.38 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

130 µm/m·K72.2 µin/in·°F
110 µm/m·K61.1 µin/in·°F
80 µm/m·K44.4 µin/in·°F
130 µm/m·K72.2 µin/in·°F

Max Service Temperature (continuous)

65°C149 °F
55°C131 °F
95°C203 °F
70°C158 °F

Min Service Temperature

-40°C-40 °F
-30°C-22 °F
-40°C-40 °F
-40°C-40 °F

Heat Deflection Temp. @ 0.45 MPa

70°C158 °F
68°C154 °F
120°C248 °F
75°C167 °F

Heat Deflection Temp. @ 1.8 MPa

55°C131 °F
52°C126 °F
95°C203 °F
58°C136 °F

Vicat Softening Point (B50)

75°C167 °F
75°C167 °F
140°C284 °F
100°C212 °F

Limiting Oxygen Index

19%
19%
20%

Max Service Temperature (short-term)

90°C194 °F
85°C185 °F
140°C284 °F
95°C203 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹⁰ Ω·m3.94×10¹⁷ µΩ·in
1×10¹¹ Ω·m3.94×10¹⁸ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in

Dielectric Strength

18 kV/mm457 V/mil
16 kV/mm406 V/mil
16 kV/mm406 V/mil
16 kV/mm406 V/mil

Dielectric Constant (1 MHz)

4
6
3.4
3.4

Dissipation Factor (1 MHz)

0.04
0.09
0.025
0.03

Volume Resistivity

1×10¹² Ω·cm
1×10¹³ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁴ Ω·cm

Surface Resistivity

1×10¹³ Ω
1×10¹³ Ω
1×10¹⁴ Ω

Comparative Tracking Index (CTI)

600 V
600 V
600 V

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

55 / 100
45 / 100
50 / 100

UV / Weathering Resistance

50 / 100
12 / 100
45 / 100
70 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

75 / 100
85 / 100
65 / 100
75 / 100

Weldability

55 / 100
70 / 100
60 / 100
60 / 100

Formability (cold)

78 / 100
80 / 100
70 / 100
80 / 100

Polishability

85 / 100
92 / 100
80 / 100
85 / 100

Mold Shrinkage

0.5%
0.5%
0.5%

Processing Melt Temperature (typ.)

200°C392 °F
245°C473 °F
200°C392 °F

Mold Temperature (typ.)

55°C131 °F
70°C158 °F
55°C131 °F

Melt Flow Rate

10 g/10 min

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

100 MJ/kg42,992 BTU/lb
95 MJ/kg40,843 BTU/lb
105 MJ/kg45,142 BTU/lb
105 MJ/kg45,142 BTU/lb

Embodied Carbon (primary production)

4 kg CO₂/kg
4.5 kg CO₂/kg
4.5 kg CO₂/kg
4.5 kg CO₂/kg

Embodied Water

350 L/kg41.9 gal/lb
250 L/kg30 gal/lb
600 L/kg71.9 gal/lb
500 L/kg59.9 gal/lb

Typical Recycled Content

2%
0%
2%
0%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

31 kN·m/kg
38 kN·m/kg
54 kN·m/kg
27 kN·m/kg

Specific Stiffness (E / density)

1.2 MN·m/kg
1.3 MN·m/kg
2.5 MN·m/kg
1.2 MN·m/kg

Modulus of Resilience

383 kJ/m³
490 kJ/m³
473 kJ/m³
280 kJ/m³

Same in both: Thermal Diffusivity 0.1 mm²/s · Thermal Shock Resistance Index 0

Strength versus weight

Yield strength against density for every polymer grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

0.1110100123Density (g/cm³)Yield strength (MPa) — log scaleCNCTACACAB

Manufacturing and finishing

CapabilityCACNCTACAB
Default condition
Relative cost$$$ Premium$$$ Premium$$$ Premium$$$ Premium
Min. machined wall
Best machined surface

Ready to make it?

Upload a CAD file and FabDigit prices the part in CA and CN side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.