FabDigit

Fused Silica vs N-BK7 and 2 more: properties

Fused SilicaN-BK7SapphireCaF2

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

72 GPa10.4 Msi
82 GPa11.9 Msi
400 GPa58 Msi
75.8 GPa11 Msi

Shear Modulus

31 GPa4.5 Msi
34 GPa4.9 Msi
148 GPa21.5 Msi
33.8 GPa4.9 Msi

Bulk Modulus

37 GPa5.4 Msi
47 GPa6.7 Msi
250 GPa36.3 Msi
83 GPa12 Msi

Poisson's Ratio

0.17
0.21
0.27
0.26

Tensile Strength (Ultimate)

50 MPa7.3 ksi
50 MPa7.3 ksi
400 MPa58 ksi
37 MPa5.4 ksi

Elongation at Break

0%
0%
0%

Compressive Strength

1,150 MPa167 ksi
1,000 MPa145 ksi
2,000 MPa290 ksi

Flexural Strength

67 MPa9.7 ksi
65 MPa9.4 ksi
760 MPa110 ksi
37 MPa5.4 ksi

Shear Strength

30 MPa4.4 ksi
40 MPa5.8 ksi
350 MPa50.8 ksi

Fracture Toughness (K_IC)

0.75 MPa·√m0.68 ksi·√in
0.85 MPa·√m0.77 ksi·√in
2.2 MPa·√m2 ksi·√in
0.33 MPa·√m0.3 ksi·√in

Hardness, Vickers

700 HV
610 HV
2,000 HV
165 HV

Hardness, Knoop

560 HK
610 HK
2,000 HK
158 HK

Hardness, Mohs

6
6
9
4

Physical

Density and transition temperatures.

Density

2.2 g/cm³0.08 lb/in³
2.51 g/cm³0.09 lb/in³
3.98 g/cm³0.14 lb/in³
3.18 g/cm³0.11 lb/in³

Melting Point (Solidus)

1,713°C3,115 °F
2,053°C3,727 °F
1,418°C2,584 °F

Refractive Index

1.459
1.517
1.768
1.434

Light Transmission

92%
92%
85%
94%

Same in both: Porosity 0%

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

1.4 W/m·K0.8 BTU/hr·ft·°F
1.1 W/m·K0.64 BTU/hr·ft·°F
27 W/m·K15.6 BTU/hr·ft·°F
9.7 W/m·K5.6 BTU/hr·ft·°F

Specific Heat Capacity

740 J/kg·K0.18 BTU/lb·°F
858 J/kg·K0.2 BTU/lb·°F
761 J/kg·K0.18 BTU/lb·°F
854 J/kg·K0.2 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

0.55 µm/m·K0.31 µin/in·°F
7.1 µm/m·K3.9 µin/in·°F
5.8 µm/m·K3.2 µin/in·°F
18.9 µm/m·K10.5 µin/in·°F

Max Service Temperature (continuous)

1,100°C2,012 °F
500°C932 °F
1,800°C3,272 °F
800°C1,472 °F

Min Service Temperature

-200°C-328 °F
-200°C-328 °F
-269°C-452 °F
-200°C-328 °F

Electrical

Conductivity and insulation.

Electrical Resistivity

1×10¹⁶ Ω·m3.94×10²³ µΩ·in
1×10¹² Ω·m3.94×10¹⁹ µΩ·in
1×10¹⁴ Ω·m3.94×10²¹ µΩ·in
1×10¹⁴ Ω·m3.94×10²¹ µΩ·in

Dielectric Strength

30 kV/mm762 V/mil
15 kV/mm381 V/mil
17 kV/mm432 V/mil

Dielectric Constant (1 MHz)

3.8
7
9.8
6.76

Dissipation Factor (1 MHz)

1×10⁻⁴
1×10⁻⁴

Volume Resistivity

1×10¹⁸ Ω·cm
1×10¹⁴ Ω·cm
1×10¹⁶ Ω·cm
1×10¹⁶ Ω·cm

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Corrosion Resistance

95 / 100
78 / 100
95 / 100
45 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

10 / 100
18 / 100
5 / 100
45 / 100

Polishability

98 / 100
95 / 100
98 / 100
60 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

55 MJ/kg23,646 BTU/lb
30 MJ/kg12,898 BTU/lb
400 MJ/kg171,969 BTU/lb

Embodied Carbon (primary production)

4 kg CO₂/kg
2 kg CO₂/kg
60 kg CO₂/kg

Embodied Water

80 L/kg9.6 gal/lb
90 L/kg10.8 gal/lb
250 L/kg30 gal/lb

Typical Recycled Content

0%
5%
5%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

23 kN·m/kg
20 kN·m/kg
101 kN·m/kg
12 kN·m/kg

Specific Stiffness (E / density)

32.7 MN·m/kg
32.7 MN·m/kg
100.5 MN·m/kg
23.8 MN·m/kg

Thermal Diffusivity

0.8 mm²/s
0.5 mm²/s
8.9 mm²/s
3.6 mm²/s

Thermal Shock Resistance Index

2
0
5
0

Strength versus weight

Yield strength against density for every glass grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

501002005002.533.5Density (g/cm³)Yield strength (MPa) — log scaleN-BK7Fused SilicaSapphire

Manufacturing and finishing

CapabilityFused SilicaN-BK7SapphireCaF2
Default conditionAnnealed GlassAnnealed GlassAnnealed Glass
Relative cost$$ Standard$$ Standard$$ Standard$$$$ High
Min. machined wall
Best machined surface

Ready to make it?

Upload a CAD file and FabDigit prices the part in Fused Silica and N-BK7 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.