8079800680118090

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

69 GPa10 Msi
69 GPa10 Msi
69 GPa10 Msi
78 GPa11.3 Msi

Shear Modulus

26 GPa3.8 Msi
26 GPa3.8 Msi
26 GPa3.8 Msi
29 GPa4.2 Msi

Bulk Modulus

70 GPa10.2 Msi
70 GPa10.2 Msi
69 GPa10 Msi
76 GPa11 Msi

Poisson's Ratio

0.33
0.33
0.33
0.34

Tensile Strength (Ultimate)

85 MPa12.3 ksi
155 MPa22.5 ksi
145 MPa21 ksi
480 MPa69.6 ksi

Yield Strength (0.2% offset)

35 MPa5.1 ksi
130 MPa18.9 ksi
120 MPa17.4 ksi
425 MPa61.6 ksi

Elongation at Break

25%
10%
4%
6%

Shear Strength

55 MPa8 ksi
95 MPa13.8 ksi
90 MPa13.1 ksi
290 MPa42.1 ksi

Fatigue Strength (Endurance Limit)

35 MPa5.1 ksi
55 MPa8 ksi
55 MPa8 ksi
155 MPa22.5 ksi

Hardness, Brinell

22 HB
45 HB
42 HB
135 HB

Hardness, Vickers

46 HV

Compressive Strength

440 MPa63.8 ksi

Fracture Toughness (K_IC)

32 MPa·√m29.1 ksi·√in

Physical

Density and transition temperatures.

Density

2.72 g/cm³0.1 lb/in³
2.71 g/cm³0.1 lb/in³
2.71 g/cm³0.1 lb/in³
2.54 g/cm³0.09 lb/in³

Melting Point (Solidus)

645°C1,193 °F
630°C1,166 °F
620°C1,148 °F
600°C1,112 °F

Same in both: Liquidus Temperature 655°C1,211 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

225 W/m·K130 BTU/hr·ft·°F
185 W/m·K107 BTU/hr·ft·°F
205 W/m·K118 BTU/hr·ft·°F
93 W/m·K53.7 BTU/hr·ft·°F

Specific Heat Capacity

900 J/kg·K0.21 BTU/lb·°F
900 J/kg·K0.21 BTU/lb·°F
900 J/kg·K0.21 BTU/lb·°F
930 J/kg·K0.22 BTU/lb·°F

Thermal Expansion (CTE, 20–100 °C)

23.6 µm/m·K13.1 µin/in·°F
23.6 µm/m·K13.1 µin/in·°F
23.4 µm/m·K13 µin/in·°F
21.4 µm/m·K11.9 µin/in·°F

Latent Heat of Fusion

395 J/g170 BTU/lb
390 J/g168 BTU/lb
395 J/g170 BTU/lb
390 J/g168 BTU/lb

Max Service Temperature (continuous)

150°C302 °F
120°C248 °F
150°C302 °F
120°C248 °F

Min Service Temperature

-196°C-321 °F
-196°C-321 °F
-196°C-321 °F
-253°C-423 °F

Electrical

Conductivity and insulation.

Electrical Conductivity

58 % IACS
47 % IACS
45 % IACS
23 % IACS

Electrical Resistivity

2.97×10⁻⁸ Ω·m1.17 µΩ·in
3.7×10⁻⁸ Ω·m1.46 µΩ·in
3.8×10⁻⁸ Ω·m1.5 µΩ·in
7.5×10⁻⁸ Ω·m2.95 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.83 V
-0.78 V
-0.84 V
-0.8 V

Corrosion Resistance

72 / 100
62 / 100
65 / 100
40 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

30 / 100
35 / 100
30 / 100
55 / 100

Machinability Rating (AISI 1212 = 100 %)

30%
30%
30%
45%

Weldability

75 / 100
70 / 100
60 / 100
25 / 100

Formability (cold)

95 / 100
78 / 100
60 / 100
20 / 100

Castability

60 / 100

Brazeability / Solderability

55 / 100
70 / 100
55 / 100
15 / 100

Polishability

50 / 100
40 / 100
45 / 100
55 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

200 MJ/kg85,985 BTU/lb
200 MJ/kg85,985 BTU/lb
200 MJ/kg85,985 BTU/lb
220 MJ/kg94,583 BTU/lb

Embodied Carbon (primary production)

12.5 kg CO₂/kg
12 kg CO₂/kg
12 kg CO₂/kg
14 kg CO₂/kg

Embodied Water

1,200 L/kg144 gal/lb
1,150 L/kg138 gal/lb
1,200 L/kg144 gal/lb
1,200 L/kg144 gal/lb

Typical Recycled Content

25%
35%
35%
5%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

31 kN·m/kg
57 kN·m/kg
54 kN·m/kg
189 kN·m/kg

Specific Stiffness (E / density)

25.4 MN·m/kg
25.5 MN·m/kg
25.5 MN·m/kg
30.7 MN·m/kg

Modulus of Resilience

9 kJ/m³
122 kJ/m³
104 kJ/m³
1,158 kJ/m³

Thermal Diffusivity

91.9 mm²/s
75.9 mm²/s
84.1 mm²/s
39.4 mm²/s

Thermal Shock Resistance Index

12
18
18
27

Strength versus weight

Yield strength against density for every aluminum grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

20501002005002.22.42.62.83Density (g/cm³)Yield strength (MPa) — log scale8006801180798090

Manufacturing and finishing

Capability8079800680118090
CNC machiningYes
Default conditionT851
Relative cost$ Budget$ Budget$ Budget$$$$ High
Min. machined wall0.5 mm
Best machined surfaceRa 0.8 µm
DLCYes

Both are offered for Sheet metal. They share 15 finishes: Anodizing Type II, Cerakote, Chem Film (Alodine), E-Coating, Electroless Nickel (EN), Electropolishing, Epoxy Coating, Gold Plating, Hard Anodize Type III w/ PTFE, Hard Anodizing Type III, Nickel Plating, PTFE Coating and 3 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 8079 and 8006 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.

Typical handbook values for the conditions named above, normalised for comparison. Hardness on non-Brinell scales is converted approximately for charting only. Request certified data with your order for design-critical properties.