FabDigit

3004 vs 3003 and 2 more: properties

3004300330053103

Mechanical

Strength, stiffness, ductility and hardness at room temperature.

Elastic (Young's) Modulus

69 GPa10 Msi
68.9 GPa10 Msi
69 GPa10 Msi
69 GPa10 Msi

Shear Modulus

26 GPa3.8 Msi
25 GPa3.6 Msi
26 GPa3.8 Msi
26 GPa3.8 Msi

Bulk Modulus

72 GPa10.4 Msi
69 GPa10 Msi
70 GPa10.2 Msi
69 GPa10 Msi

Tensile Strength (Ultimate)

240 MPa34.8 ksi
150 MPa21.8 ksi
175 MPa25.4 ksi
150 MPa21.8 ksi

Yield Strength (0.2% offset)

200 MPa29 ksi
145 MPa21 ksi
155 MPa22.5 ksi
130 MPa18.9 ksi

Elongation at Break

12%
10%
5%
7%

Compressive Strength

205 MPa29.7 ksi

Shear Strength

125 MPa18.1 ksi
96 MPa13.9 ksi
105 MPa15.2 ksi
97 MPa14.1 ksi

Fatigue Strength (Endurance Limit)

105 MPa15.2 ksi
62 MPa9 ksi
65 MPa9.4 ksi
62 MPa9 ksi

Hardness, Brinell

63 HB
40 HB
48 HB
42 HB

Hardness, Vickers

47 HV

Same in both: Poisson's Ratio 0.33

Physical

Density and transition temperatures.

Density

2.72 g/cm³0.1 lb/in³
2.73 g/cm³0.1 lb/in³
2.73 g/cm³0.1 lb/in³
2.73 g/cm³0.1 lb/in³

Melting Point (Solidus)

629°C1,164 °F
643°C1,189 °F
630°C1,166 °F
645°C1,193 °F

Liquidus Temperature

654°C1,209 °F
654°C1,209 °F
655°C1,211 °F
655°C1,211 °F

Thermal

How each material carries heat and how hot it can run.

Thermal Conductivity

162 W/m·K93.6 BTU/hr·ft·°F
159 W/m·K91.9 BTU/hr·ft·°F
163 W/m·K94.2 BTU/hr·ft·°F
160 W/m·K92.4 BTU/hr·ft·°F

Thermal Expansion (CTE, 20–100 °C)

23.2 µm/m·K12.9 µin/in·°F
23.2 µm/m·K12.9 µin/in·°F
23.8 µm/m·K13.2 µin/in·°F
23.2 µm/m·K12.9 µin/in·°F

Latent Heat of Fusion

393 J/g169 BTU/lb
390 J/g168 BTU/lb
397 J/g171 BTU/lb
390 J/g168 BTU/lb

Max Service Temperature (continuous)

150°C302 °F
150°C302 °F
120°C248 °F
120°C248 °F

Min Service Temperature

-196°C-321 °F
-196°C-321 °F
-200°C-328 °F
-196°C-321 °F

Same in both: Specific Heat Capacity 893 J/kg·K0.21 BTU/lb·°F

Electrical

Conductivity and insulation.

Electrical Conductivity

42 % IACS
41 % IACS
41 % IACS
42 % IACS

Electrical Resistivity

4.1×10⁻⁸ Ω·m1.61 µΩ·in
4.2×10⁻⁸ Ω·m1.65 µΩ·in
4.2×10⁻⁸ Ω·m1.65 µΩ·in
4.1×10⁻⁸ Ω·m1.61 µΩ·in

Chemical & Environmental

Corrosion and environmental resistance (0–100 scores).

Galvanic Potential (seawater, vs SCE)

-0.84 V
-0.83 V
-0.84 V
-0.83 V

Corrosion Resistance

68 / 100
68 / 100
68 / 100
70 / 100

Manufacturability

FabDigit workshop ratings (0–100 scores) — how each material behaves on the machine.

Machinability

50 / 100
45 / 100
35 / 100
35 / 100

Machinability Rating (AISI 1212 = 100 %)

90%
30%
30%

Weldability

88 / 100
90 / 100
85 / 100
90 / 100

Formability (cold)

65 / 100
70 / 100
70 / 100
65 / 100

Brazeability / Solderability

45 / 100
90 / 100
55 / 100
75 / 100

Polishability

55 / 100
45 / 100
45 / 100
50 / 100

Sustainability

Primary-production footprint per kilogram.

Embodied Energy (primary production)

200 MJ/kg85,985 BTU/lb
205 MJ/kg88,134 BTU/lb
200 MJ/kg85,985 BTU/lb
200 MJ/kg85,985 BTU/lb

Embodied Carbon (primary production)

12.5 kg CO₂/kg
12.5 kg CO₂/kg
12.5 kg CO₂/kg
12 kg CO₂/kg

Embodied Water

1,200 L/kg144 gal/lb
1,100 L/kg132 gal/lb
1,200 L/kg144 gal/lb
1,200 L/kg144 gal/lb

Typical Recycled Content

55%
35%
35%
35%

Common Calculations

Ratios derived from the values above.

Specific Strength (UTS / density)

88 kN·m/kg
55 kN·m/kg
64 kN·m/kg
55 kN·m/kg

Specific Stiffness (E / density)

25.4 MN·m/kg
25.2 MN·m/kg
25.3 MN·m/kg
25.3 MN·m/kg

Modulus of Resilience

290 kJ/m³
153 kJ/m³
174 kJ/m³
122 kJ/m³

Thermal Diffusivity

66.7 mm²/s
65.2 mm²/s
66.9 mm²/s
65.6 mm²/s

Thermal Shock Resistance Index

24
15
17
15

Strength versus weight

Yield strength against density for every aluminum grade in the FabDigit library; the compared grades are highlighted. Up and left is stronger for its weight.

20501002005002.22.42.62.83Density (g/cm³)Yield strength (MPa) — log scale3003300430053103

Manufacturing and finishing

Capability3004300330053103
CNC machiningYes
Default condition
Relative cost$ Budget$ Budget$ Budget$ Budget
Min. machined wall0.5 mm
Best machined surfaceRa 0.8 µm
DLCYes

Both are offered for Sheet metal. They share 15 finishes: Anodizing Type II, Cerakote, Chem Film (Alodine), E-Coating, Electroless Nickel (EN), Electropolishing, Epoxy Coating, Gold Plating, Hard Anodize Type III w/ PTFE, Hard Anodizing Type III, Nickel Plating, PTFE Coating and 3 more.

Ready to make it?

Upload a CAD file and FabDigit prices the part in 3004 and 3003 side by side — material, machining time, tolerance and finish in one quote. Certified material data ships with the order on request.